A molded ultra-microporous metal-organic framework material and its preparation method and application in selectively adsorbing sulfur hexafluoride

Ultramicroporous metal-organic frame materials prepared by wet granulation method solve the problem of separation of SF6 and CF4 in the prior art, achieve the separation effect of high selectivity and high adsorption capacity, and overcome the application difficulties of powder materials , high purity gas and good mechanical properties were obtained.

CN116586037BActive Publication Date: 2024-11-12ZHEJIANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310462676.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-26
Publication Date
2024-11-12
Estimated Expiration
2043-04-26

AI Technical Summary

Technical Problem

The prior art is difficult to efficiently separate and purify greenhouse gases such as sulfur hexafluoride (SF6) and carbon tetrafluoride (CF4), especially at low concentrations, and it is difficult to take into account the selectivity and adsorption capacity of conventional solid porous adsorbents. In actual applications, there are problems with dust pollution and structural stability of materials.

Method used

Wet granulation method is used to prepare molded ultramicroporous metal-organic frame materials, and the material with infinitely extended one-dimensional square pores is formed through the coordination reaction of specific metal ions and fumaric acid derivatives, and the material is improved by combining polyhydroxy binders. The stability and mechanical properties of the system achieve high selectivity and high adsorption capacity SF6/N2 or SF6/CF4 separation.

Benefits of technology

It achieves efficient adsorption and selective separation of sulfur hexafluoride, obtains high-purity nitrogen or carbon tetrafluoride gas, overcomes the dust pollution and structural stability of powder materials, and has excellent mechanical properties and recycling capabilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116586037B_ABST
    Figure CN116586037B_ABST
Patent Text Reader

Abstract

The present invention provides a molded ultra-microporous metal-organic framework material, a preparation method thereof, and an application of selectively adsorbing sulfur hexafluoride, and relates to the technical field of chemical engineering. The present invention wet-granulates an ultra-microporous metal-organic framework material, a binder, and water to obtain a molded ultra-microporous metal-organic framework material; the binder is one or more of hydroxyethyl cellulose, hydroxypropyl cellulose, polyvinyl alcohol, polyvinyl butyral, and kaolin; the ultra-microporous metal-organic framework material is prepared by mixing a soluble metal salt, an organic ligand, an alkali, and water through a coordination reaction; the metal ion in the soluble metal salt is Cr 3+ 、Al 3+ 、V 3+ and Fe 3+ The organic ligand is fumaric acid or a fumaric acid derivative. The molded ultra-microporous metal-organic framework material prepared by the present invention has high SF6 adsorption capacity and good selectivity, and can achieve effective separation of SF6 / N2 or SF6 / CF4.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chemical engineering, and in particular to a molded ultra-microporous metal-organic framework material, a preparation method thereof, and an application thereof in selectively adsorbing sulfur hexafluoride. Background Art

[0002] Sulfur hexafluoride (SF6) is the most potent greenhouse gas, with a global warming potential about 23,900 times greater than that of carbon dioxide (CO2), and it can remain in the atmosphere for up to 3,200 years. Because SF6 is non-toxic and has excellent dielectric and arc-extinguishing properties, it is also widely used in the electronics industry. Pure SF6 gas is expensive, so industry usually mixes SF6 with a certain proportion of nitrogen (N2) to maintain dielectric properties comparable to pure SF6 while reducing the cost of use. Accordingly, efficient separation and recovery of SF6 from scrapped devices or industrial exhaust gases is essential to improving overall economic benefits and environmental sustainability.

[0003] In addition to SF6, another greenhouse gas, carbon tetrafluoride (CF4), is also one of the most widely used plasma etching gases in the electronics industry. It is mainly used for etching thin film materials such as silicon, silicon dioxide, and silicon nitride. It is also used for electronic device surface cleaning, low-temperature refrigeration, gas insulation, etc. The fluorocarbon direct synthesis method is the main method for preparing CF4 in industry. However, the crude CF4 product obtained by this method also contains impurity components such as hydrofluoric acid (HF), fluorine gas (F2), and sulfur hexafluoride (SF6), which cannot meet the use standards of electronic grade CF4. Therefore, CF4 needs to be further purified to a purity of more than 99.999%. Among them, acidic impurities such as HF and F2 can be removed by water washing and alkaline washing, while SF6 and CF4 have similar properties (both are relatively inert), and have similar molecular shapes and sizes (molecular dynamic diameters are 2.3 and 1.7, respectively). and ), whose separation is extremely challenging.

[0004] In industry, the difference in boiling points between SF6 and other gases is used to achieve effective separation of SF6 / N2 or SF6 / CF4 through low-temperature distillation, liquefaction, etc. However, the temperature change process involved in these technologies requires a lot of energy consumption, which is very uneconomical, especially when the SF6 concentration is low. In contrast, adsorption separation technology that does not involve phase change processes is more energy-efficient and clean, and has more significant advantages in separating low-concentration SF6. Conventional solid porous adsorbents show a certain SF6 adsorption capacity, such as molecular sieve materials MFI-1 and MFI-2 (pore size The adsorption capacity of 13X molecular sieve (pore size) at 25 °C and 10 kPa is 0.86 mmol / g and 0.70 mmol / g respectively (Journal of Industrial and Engineering Chemistry, 2018, 62: 64-71). ) can also achieve an SF6 adsorption capacity of 0.97mmol / g (Chemical Engineering Journal, 2015, 262: 683-690). However, due to the lack of diversity in their pore structures, it is difficult for these materials to significantly improve their affinity for SF6, and the adsorption capacity is still not high enough. At the same time, since the molecular sizes of these gases are similar, for example, the molecular kinetic diameters of SF6 and CF4 differ by only Conventional adsorption materials are difficult to achieve high-selectivity separation. Therefore, it is urgent to develop new and efficient adsorption materials and adsorption separation methods.

[0005] In recent years, metal-organic framework materials (MOFs) have shown great potential in the field of gas separation due to their diverse pore structures and fine controllability. However, for SF6 / N2 or SF6 / CF4 separation, the MOFs reported so far still have the problem of difficulty in balancing selectivity and adsorption capacity. Moreover, these MOFs are all powder materials, and in actual use, there are many problems such as dust pollution, excessive pressure drop in the adsorption tower bed, pipeline blockage, and transportation difficulties. After these powder materials are formed, their selectivity and adsorption capacity are usually further reduced due to pore blockage and partial collapse of the skeleton structure. Summary of the invention

[0006] In view of this, the present invention aims to provide a molded ultra-microporous metal-organic framework material and a preparation method thereof and an application of selectively adsorbing sulfur hexafluoride. The molded ultra-microporous metal-organic framework material prepared by the present invention has a high adsorption capacity for SF6 and good selectivity, and can achieve effective separation of SF6 / N2 or SF6 / CF4.

[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0008] The present invention provides a method for preparing a molded ultra-microporous metal-organic framework material, comprising the following steps:

[0009] The ultra-microporous metal-organic framework material, a binder and water are mixed and wet granulated to obtain the molded ultra-microporous metal-organic framework material; the binder is one or more of hydroxyethyl cellulose, hydroxypropyl cellulose, polyvinyl alcohol, polyvinyl butyral and kaolin;

[0010] The ultra-microporous metal-organic framework material is prepared by mixing a soluble metal salt, an organic ligand, a base and water through a coordination reaction; the metal ion in the soluble metal salt is Cr 3+ 、Al 3+ 、V 3+ and Fe 3+ One or more of the following; the organic ligand is fumaric acid or a fumaric acid derivative.

[0011] Preferably, the mass of the binder is 0.1-15% of the sum of the mass of the binder and the ultra-microporous metal-organic framework material.

[0012] Preferably, the particle size of the molded ultra-microporous metal-organic framework material is 1 to 2 mm.

[0013] Preferably, the fumaric acid derivative has a structure as shown in Formula I:

[0014]

[0015] In formula I, R1 and R2 are independently selected from H, F, Cl, Br, I or CH3, and R1 and R2 are not H at the same time.

[0016] Preferably, the base is sodium hydroxide; the molar ratio of the metal ions in the organic ligand and the soluble metal salt to the base is 1-2:2:4-8.

[0017] Preferably, the ultra-microporous metal-organic framework material has infinitely extended periodic one-dimensional square channels with a pore size of

[0018] The present invention provides a molded ultra-microporous metal-organic framework material prepared by the preparation method described in the above technical solution.

[0019] The present invention provides the application of the molded ultra-microporous metal-organic framework material described in the above technical solution to selectively adsorb sulfur hexafluoride from a mixed gas; the mixed gas includes sulfur hexafluoride and nitrogen or sulfur hexafluoride and carbon tetrafluoride.

[0020] Preferably, the volume ratio of sulfur hexafluoride to nitrogen or sulfur hexafluoride to carbon tetrafluoride in the mixed gas is 99:1 to 1:99.

[0021] Preferably, the adsorption is one or more of fixed bed adsorption, fluidized bed adsorption and moving bed adsorption; the temperature of the adsorption is -20 to 60°C, and the pressure is 0.5 to 10 bar.

[0022] The invention provides a method for preparing a molded ultra-microporous metal-organic framework material, comprising the following steps: mixing an ultra-microporous metal-organic framework material, a binder and water for wet granulation to obtain the molded ultra-microporous metal-organic framework material; the binder is one or more of hydroxyethyl cellulose, hydroxypropyl cellulose, polyvinyl alcohol, polyvinyl butyral and kaolin; the ultra-microporous metal-organic framework material is prepared by mixing a soluble metal salt, an organic ligand, an alkali and water through a coordination reaction; the metal ion in the soluble metal salt is Cr 3+ 、Al 3+ 、V 3+ and Fe 3+ One or more of; the organic ligand is fumaric acid or a fumaric acid derivative. The present invention synthesizes ultra-microporous metal-organic framework materials with specific metal ions and carboxylic acid organic ligands of specific sizes. Compared with conventional adsorbents and other MOFs materials, the ultra-microporous metal-organic framework materials have stronger SF6 affinity (the adsorption capacity of SF6 under equilibrium conditions is significantly higher than that of N2 or CF4) and significantly improved SF6 selectivity, and can achieve effective separation of sulfur hexafluoride and nitrogen mixed gas (SF6 / N2) or sulfur hexafluoride and carbon tetrafluoride mixed gas (SF6 / CF4); the present invention prepares the molded ultra-microporous metal-organic framework materials by granulation with a specific binder, and the molded materials still maintain almost the same specific surface area and SF6 adsorption and separation performance as the original metal-organic framework materials, and have complete surface morphology and excellent mechanical properties, overcoming many problems of dust pollution, excessive pressure drop of the adsorption tower bed, pipeline blockage, transportation difficulties, etc., existing in the currently used powder materials. In addition, the present invention also significantly improves the stability of the formed ultra-microporous metal-organic framework material through the hydrogen bond interaction between the polyhydroxy binder and the ultra-microporous metal-organic framework material. At the same time, the preparation method provided by the present invention has outstanding advantages such as mild operating conditions, energy saving and environmental protection, and small equipment investment, and the raw material cost of the material is low, which is expected to bring economic benefits to small and medium-sized enterprises.

[0023] The present invention provides a molded ultra-microporous metal-organic framework material prepared by the preparation method described in the above technical solution. The molded ultra-microporous metal-organic framework material provided by the present invention has the advantages of large sulfur hexafluoride adsorption capacity, high selectivity, and recyclability, and has excellent stability, and a thermal decomposition temperature of nearly 400°C. The molded ultra-microporous metal-organic framework material is used to selectively adsorb sulfur hexafluoride from a mixture of sulfur hexafluoride and nitrogen or a mixture of sulfur hexafluoride and carbon tetrafluoride, and nitrogen or carbon tetrafluoride gas with a purity of up to 99.999% and sulfur hexafluoride gas with a purity of up to 99.99% can be obtained at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1The adsorption isotherms of the ultra-microporous metal-organic framework material Al(fum) obtained in Example 1 for SF6, CF4 and N2 at 298K;

[0025] Figure 2 The adsorption isotherms of the ultra-microporous metal-organic framework material Al(fum) obtained in Example 1 for SF6, CF4 and N2 at 273K;

[0026] Figure 3 The fixed bed penetration curves of the ultra-microporous metal-organic framework material Al(fum) in Example 2 for SF6 / N2 (volume ratio 10:90) mixed gas and SF6 / CF4 (volume ratio 4:96) mixed gas at 273K and 298K; Figure 3 A is a fixed bed penetration curve for SF6 / N2 (volume ratio 10:90) mixed gas, and B is a fixed bed penetration curve for SF6 / CF4 (volume ratio 4:96) mixed gas;

[0027] Figure 4 It is a fixed bed desorption curve diagram of the ultra-microporous metal-organic framework material Al(fum) in Example 2 after adsorption saturation of SF6 / N2 (volume ratio 10:90) mixed gas and SF6 / CF4 (volume ratio 4:96) mixed gas at 298K; Figure 4 In the figure, A is a fixed bed desorption curve diagram after SF6 / N2 (volume ratio 10:90) mixed gas adsorption saturation, and B is a fixed bed desorption curve diagram after SF6 / CF4 (volume ratio 4:96) mixed gas adsorption saturation;

[0028] Figure 5 The SF6 dynamic adsorption capacity of the ultra-microporous metal-organic framework material Al(fum) in Example 2 after 5 adsorption-desorption cycles of SF6 / N2 (volume ratio 10:90) mixed gas at 298K;

[0029] Figure 6 A comparison diagram of the morphologies of the molded materials obtained by molding the ultra-microporous metal-organic framework material with different binders in Example 3; Figure 6 Among them, A is Al(fum)@5%HPC, B is Al(fum)@2%HPC, C is Al(fum)@5%PVA, D is Al(fum)@2%PVA, E is Al(fum)@10%sucrose, and F is Al(fum)@5%sucrose;

[0030] Figure 7 Thermogravimetric curves of the formed ultra-microporous materials Al(fum)@2%HPC and Al(fum)@5%HPC obtained in Example 4 and Example 5;

[0031] Figure 8Thermogravimetric curves of the molded ultra-microporous materials Al(fum)@2%PVA and Al(fum)@5%PVA obtained in Example 6 and Example 7;

[0032] Fig. 9 X-ray diffraction patterns of the ultra-microporous materials obtained in Examples 4, 5, 6 and 7;

[0033] Fig.10 The adsorption isotherms of N2 at 77K for the formed ultra-microporous materials Al(fum)@2%HPC and Al(fum)@2%PVA obtained in Example 4 and Example 6; Fig.10 A is the adsorption isotherm of Al(fum)@2%HPC for N2 at 77K, and B is the adsorption isotherm of Al(fum)@2%PVA for N2 at 77K.

[0034] Fig.11 The wear test effect diagram of the formed ultra-microporous materials obtained in Example 4, Example 5, Example 6 and Example 7;

[0035] Fig.12 This is the adsorption isotherm diagram of the molded ultra-microporous material Al(fum)@2%HPC obtained in Example 4 for SF6, CF4 and N2 at 298K;

[0036] Fig.13 The fixed bed penetration curves of the ultra-microporous material Al(fum)@2%HPC formed in Example 8 for SF6 / N2 (volume ratio 10:90) mixed gas and SF6 / CF4 (volume ratio 4:96) mixed gas at 273K and 298K; Fig.13 A is a fixed bed penetration curve for SF6 / N2 (volume ratio 10:90) mixed gas, and B is a fixed bed penetration curve for SF6 / CF4 (volume ratio 4:96) mixed gas;

[0037] Fig.14 It is a fixed bed desorption curve diagram of the ultra-microporous material Al(fum)@2%HPC formed in Example 8 after adsorption saturation of SF6 / N2 (volume ratio 10:90) mixed gas and SF6 / CF4 (volume ratio 4:96) mixed gas at 298K; Fig.14 A is a fixed bed desorption curve after SF6 / N2 (volume ratio 10:90) mixed gas adsorption saturation, B is a fixed bed desorption curve after SF6 / CF4 (volume ratio 4:96) mixed gas adsorption saturation;

[0038] Fig.15This is a graph of the dynamic adsorption capacity of SF6 for the ultra-microporous material Al(fum)@2%HPC formed in Example 8 after four adsorption-desorption cycles of SF6 / N2 (volume ratio 10:90) mixed gas at 298K. DETAILED DESCRIPTION

[0039] The present invention provides a method for preparing a molded ultra-microporous metal-organic framework material, comprising the following steps:

[0040] The ultra-microporous metal-organic framework material, a binder and water are mixed and wet granulated to obtain the molded ultra-microporous metal-organic framework material; the binder is one or more of hydroxyethyl cellulose, hydroxypropyl cellulose, polyvinyl alcohol, polyvinyl butyral and kaolin;

[0041] The ultra-microporous metal-organic framework material is prepared by mixing a soluble metal salt, an organic ligand, a base and water through a coordination reaction; the metal ion in the soluble metal salt is Cr 3+ 、Al 3+ 、V 3+ and Fe 3+ One or more of the following; the organic ligand is fumaric acid or a fumaric acid derivative.

[0042] The present invention first describes the ultra-microporous metal-organic framework material.

[0043] In the present invention, the ultra-microporous metal-organic framework material is prepared by mixing a soluble metal salt, an organic ligand, a base and water through a coordination reaction. In the present invention, the metal ion in the soluble metal salt is Cr 3+ 、Al 3+ 、V 3+ and Fe 3+ One or more of the following, preferably Al 3+ , the soluble metal salt is preferably a sulfate, carbonate or nitrate of the metal ion. In the present invention, the organic ligand is fumaric acid or a fumaric acid derivative, and the fumaric acid derivative preferably has a structure shown in Formula I, in which R1 and R2 are independently selected from H, F, Cl, Br, I or CH3, and R1 and R2 are not H at the same time; in an embodiment of the present invention, the R1 and R2 are preferably independently selected from H or CH3. The present invention has no special requirements for the source of the fumaric acid derivative, and it can be prepared by using commercial products well known to those skilled in the art or by a preparation method well known to those skilled in the art. In the present invention, the base is preferably sodium hydroxide; the molar ratio of the metal ion to the base in the organic ligand and the soluble metal salt is preferably 1 to 2:2:4 to 8, and more preferably 2:2:6. The present invention has no special requirements for the amount of water used, as long as it can achieve sufficient dissolution of each component.

[0044]

[0045] In the present invention, the coordination reaction can adopt the interface slow diffusion method or the solvent stirring method. In the present invention, the specific operation of the interface slow diffusion method is preferably: mixing the organic ligand, alkali and part of the water to obtain a first mixed solution; mixing the soluble metal salt with the remaining water to obtain a second mixed solution; dropping the first mixed solution into the second mixed solution, and then standing at 0-25°C for coordination reaction; the dropping speed is preferably 2-3mL / min; the coordination reaction time (i.e., the standing time) is preferably 7-21 days. In the present invention, the specific operation of the solvent stirring method is preferably: mixing the organic ligand, alkali and part of the water to obtain a third mixed solution; mixing the soluble metal salt with the remaining water to obtain a fourth mixed solution; stirring and mixing the third mixed solution and the fourth mixed solution for coordination reaction; the temperature of the coordination reaction is preferably 25-85°C, more preferably 60°C, the time is preferably 0.1-24h, more preferably 2h, and the stirring rate is preferably 200-800r / min, more preferably 600r / min. In the present invention, after the coordination reaction is completed, the obtained coordination reaction solution is preferably filtered, the solid phase is washed with water and dried in sequence, and the drying temperature is preferably 60°C.

[0046] In the process of the coordination reaction, the metal ions (denoted as M) in the soluble metal salt aqueous solution, the organic ligands of fumaric acid and its derivatives (denoted as L) and the μ-OH provided by the base are coordinated through coordination bonds. Specifically, the metal ion M acts as a six-coordinate central node to coordinate with the four carboxyl oxygen atoms of the organic ligand L and the oxygen atoms on the two μ-OH of the base to form a MO6 spatial regular octahedral structure, and is connected through the dicarboxylic acid organic ligand L to form a periodic one-dimensional square channel with infinite extension, and the pore size is There are high-density -OH polar sites distributed on the pore surface, and the product formed by the coordination reaction (i.e., ultra-microporous metal-organic framework material) has a general structural formula represented by M(OH)L.

[0047] The present invention uses specific metal ions and specific size carboxylic acid organic ligands to synthesize ultra-microporous metal-organic framework materials, and the ultra-microporous metal-organic framework materials have a kinetic diameter close to that of SF6. The pore size can enhance the confinement effect of molecules in the confined pores, and the high-density -OH polar sites distributed on the pore surface can effectively identify the polarizability differences among SF6, N2, and CF4 molecules (the polarizability is 65.4×10 -25 cm 3 , 38.4×10 -25 cm 3 and 17.4×10-25 cm 3 ), so it can selectively and efficiently identify SF6 molecules and obtain strong affinity for them, significantly improving the adsorption and separation selectivity of the material for SF6 and N2 as well as SF6 and CF4, and achieving high selectivity and high capacity SF6 / N2 and SF6 / CF4 separation effects. For example, in an embodiment of the present invention, the ultra-microporous MOF material with the structural formula of Al(OH)(C4H2O4) (abbreviated as Al(fum)) hardly adsorbs N2 (0.24mmol / g, 298K and 100kPa conditions), while the adsorption capacity for SF6 under the corresponding conditions is as high as 3.50mmol / g, and the adsorption capacity for SF6 under low pressure reaches a record 2.77mmol / g (10kPa), and the IAST (Ideal Adsorbed Solution Theory) selectivity for SF6 / N2 mixed gas with a volume ratio of 10:90 is as high as 1610, which is much higher than other adsorbents.

[0048] Next, the method for preparing the ultra-microporous metal-organic framework material of the present invention is described in detail.

[0049] The present invention mixes the ultra-microporous metal-organic framework material, a binder and water for wet granulation to obtain the molded ultra-microporous metal-organic framework material. In the present invention, the binder is one or more of hydroxyethyl cellulose (HEC), hydroxypropyl cellulose (HPC), polyvinyl alcohol (PVA), polyvinyl butyral (PVB) and kaolin, preferably hydroxypropyl cellulose or polyvinyl alcohol. The present invention has no special requirements for the source of the binder, and commercially available products known to those skilled in the art can be used. In the present invention, the mass of the binder is preferably 0.1-15% of the sum of the mass of the binder and the ultra-microporous metal-organic framework material, more preferably 2-10%, and further preferably 2-5%; the water is preferably deionized water. In the present invention, the specific operation of the mixing is preferably: the ultra-microporous metal-organic framework material and the binder are placed in a mortar for grinding and mixing evenly, and water is added in small amounts and multiple times during the mixing, and stirred to make it into a paste. The present invention has no special requirements for the amount of water used, as long as it can become a paste. In the present invention, the wet granulation is to extrude the paste into spherical particles after it is semi-dried; the particle size of the formed ultra-microporous metal-organic framework material is preferably 1 to 2 mm. In an embodiment of the present invention, the formed ultra-microporous metal-organic framework material is expressed as M(OH)L@x%B, where B represents a binder, and x% represents the percentage of the binder mass to the total mass of the binder and the ultra-microporous metal-organic framework material.

[0050] The present invention prepares a molded ultra-microporous metal-organic framework material by granulating with a specific binder, and can still retain the porous structure, abundant action sites and excellent stability of the original ultra-microporous metal-organic framework material that matches the size of SF6, that is, it still maintains excellent SF6 adsorption and separation performance after molding. For example, in an embodiment of the present invention, an ultra-microporous MOF material with a structural formula of Al(OH)(C4H2O4) (abbreviated as Al(fum)) is molded by adding 2wt% hydroxypropyl cellulose (HPC) as a binder, and the specific surface area of ​​the particles after molding (Al(fum)@2%HPC) is basically the same as that before molding (the specific surface area of ​​Al(fum)@2%HPC after molding is 999m 2 / g, the specific surface area of ​​Al(fum) before molding is 1040m 2 / g), and under the conditions of 298K and 10kPa, the SF6 adsorption capacity of Al(fum)@2%HPC is 2.67mmol / g, which is only 3.5% lower than that of Al(fum) powder (2.77mmol / g), indicating that the formed particles still have excellent SF6 adsorption performance. In addition, the binder molding can obtain a formed particle material with complete surface morphology, suitable particle size and better mechanical properties, which provides a strong guarantee for the long-term and stable industrial application of the material.

[0051] The present invention provides a molded ultra-microporous metal-organic framework material prepared by the preparation method described in the above technical solution. The molded ultra-microporous metal-organic framework material provided by the present invention has the advantages of large sulfur hexafluoride adsorption capacity, high selectivity, recyclability, excellent stability, and a thermal decomposition temperature of nearly 400°C.

[0052] The present invention provides the use of the molded ultra-microporous metal-organic framework material described in the above technical solution to selectively adsorb sulfur hexafluoride from a mixed gas; the mixed gas includes sulfur hexafluoride and nitrogen or sulfur hexafluoride and carbon tetrafluoride. In the present invention, the volume ratio of sulfur hexafluoride to nitrogen or sulfur hexafluoride to carbon tetrafluoride in the mixed gas is preferably 99:1 to 1:99, and more preferably 4:96 to 10:90. In the present invention, when the molded ultra-microporous metal-organic framework material is used as an adsorbent and contacts a mixed gas containing sulfur hexafluoride and nitrogen or a mixed gas containing sulfur hexafluoride and carbon tetrafluoride, the adsorbent selectively adsorbs sulfur hexafluoride molecules due to the difference in molecular size and polarizability between sulfur hexafluoride and nitrogen or carbon tetrafluoride, thereby achieving separation of sulfur hexafluoride and nitrogen or sulfur hexafluoride and carbon tetrafluoride; the mixed gas may also contain impurity components such as oxygen, carbon dioxide, and moisture, which do not affect the adsorption and separation performance of the molded ultra-microporous metal-organic framework material on sulfur hexafluoride.

[0053] In the present invention, the adsorption is preferably one or more of fixed bed adsorption, fluidized bed adsorption and moving bed adsorption, preferably fixed bed adsorption; the specific operation of the fixed bed adsorption is preferably: at the set adsorption temperature and adsorption pressure, the mixed gas is passed into a fixed bed adsorption column filled with the molded ultra-microporous metal-organic framework material, the nitrogen or carbon tetrafluoride component in the mixed gas has a weak interaction with the molded ultra-microporous metal-organic framework material, the adsorption amount is relatively small, and it preferentially penetrates the bed layer, and the nitrogen or carbon tetrafluoride gas with a sulfur hexafluoride content of less than 0.01 vol% is directly obtained from the outlet of the adsorption column, and the sulfur hexafluoride component has a strong interaction with the molded ultra-microporous metal-organic framework material and is enriched in the bed layer. In the present invention, after sulfur hexafluoride is adsorbed saturated, sulfur hexafluoride-rich gas (high-purity sulfur hexafluoride gas with a purity greater than 99.99%) can be obtained by desorption. In the present invention, the adsorption temperature is preferably -20 to 60°C, and the pressure is preferably 0.5 to 10 bar; lowering the adsorption temperature is beneficial to increasing the adsorption capacity of sulfur hexafluoride, and increasing the adsorption temperature is beneficial to narrowing the temperature difference between the adsorption process and the desorption process, reducing the energy consumption required for the separation process, and increasing the diffusion rate of sulfur hexafluoride in the pores. Therefore, considering the above two factors, the adsorption temperature is further preferably 0 to 35°C, and the pressure is further preferably 1 to 5 bar. In the present invention, the desorption method can be reduced pressure and temperature desorption, temperature increase plus inert gas atmospheric pressure purge desorption or a combination of multiple desorption methods; the desorption temperature of the reduced pressure and temperature desorption is preferably 25 to 120°C, more preferably 25 to 40°C, and the desorption pressure is preferably 0.000001 to 0.1 bar, and the desorption temperature of the temperature increase plus inert gas atmospheric pressure purge desorption is preferably 25 to 120°C, more preferably 25 to 40°C.

[0054] The molded ultra-microporous metal-organic framework material provided by the present invention, its preparation method and its application in selectively adsorbing sulfur hexafluoride are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0055] Example 1

[0056] 1.05 mmol of aluminum sulfate 18hydrate (0.7 g) was weighed and dissolved in 6 mL of deionized water and preheated to 60° C., which was recorded as solution A. 2.1 mmol of fumaric acid (0.243 g) and 6.3 mmol of sodium hydroxide (0.252 g) were weighed and dissolved in 7.2 mL of deionized water and preheated to 60° C., which was recorded as solution B. The preheated solution B was mixed with the preheated solution A, stirred and reacted at 60° C. for 2 hours, and then filtered. The solid product obtained by filtration was washed with deionized water and then dried at 60° C. Finally, a white powder, i.e., an ultra-microporous metal-organic framework material, was obtained, which was recorded as Al (fum), and the yield based on aluminum was 89% (292 mg).

[0057] The synthesized powder material was placed in a vacuum degassing at 120°C for 24 hours, and the degassing pressure was less than 5 μmHg. Then, the single-component static adsorption isotherms of SF6, CF4 and N2 were tested on a Micrometrics ASAP 2460 adsorption instrument at 273K and 298K.

[0058] The adsorption isotherms of the ultra-microporous metal-organic framework Al(fum) obtained in this example for SF6, CF4 and N2 at 298K are as follows: Figure 1 As shown in the figure, the material has a high SF6 adsorption capacity (3.50mmol / g) at room temperature and pressure and almost no N2 adsorption at the same time, and the adsorption capacity of SF6 at low pressure (10kPa) reaches a record 2.77mmol / g; after calculation, the IAST (Ideal Adsorbed Solution Theory) selectivity of the material for SF6 / N2 mixed gas with a volume ratio of 10:90 is 1610. The adsorption isotherms of the ultra-microporous metal-organic framework material Al(fum) obtained in this example for SF6, CF4 and N2 at 273K are shown in the figure below: Figure 2 As shown, the material has a high SF6 adsorption capacity (3.77 mmol / g) at 273 K and 1 bar and almost no N2 adsorption.

[0059] Example 2

[0060] The ultra-microporous metal-organic framework material Al(fum) powder (0.57 g) obtained in Example 1 is loaded into a 5 cm long fixed bed adsorption column, and SF6 / N2 (volume ratio 10:90) mixed gas or SF6 / CF4 (volume ratio 4:96) mixed gas is introduced into the adsorption column at a flow rate of 2.7 mL / min at 273 K or 298 K, and high-purity N2 or CF4 (purity greater than 99.999%) is obtained in the outflowing gas; when SF6 penetrates (adsorption saturation), the adsorption is stopped, and He gas is purged at 40°C for 10 hours for desorption to obtain high-purity SF6 (purity greater than 99.99%), and the adsorption column can be recycled.

[0061] The penetration curve of the ultra-microporous metal-organic framework material Al(fum) powder in this embodiment is as follows Figure 3As shown, the mixed gas flow rate is 2.7mL / min, C represents the component concentration of the raw material at the outlet of the adsorption column, and C0 represents the initial concentration of the raw material. For the SF6 / N2 (10:90) mixed gas, the N2 component quickly penetrates at different temperatures and the retention time of the SF6 component reaches 171min / g (298K) and 190min / g (273K), indicating that the ultra-microporous metal-organic framework material has a high dynamic SF6 adsorption capacity and almost no N2 is adsorbed at the same time; for the SF6 / CF4 (4:96) mixed gas, the CF4 component quickly penetrates at different temperatures and the retention time of the SF6 component reaches 310min / g (298K) and 363min / g (273K), which also shows that the material has a high dynamic SF6 adsorption capacity. High-purity SF6 (purity greater than 99.99%) can be obtained by desorption under the conditions of 40°C and 6.0mL flow rate He gas purge. The desorption curve is shown in Figure 4 As shown, the dynamic SF6 adsorption of the material did not decrease significantly after 5 cycles (as shown in Figure 5 shown).

[0062] Example 3

[0063] Hydroxypropyl cellulose (HPC), polyvinyl alcohol (PVA) and sucrose are selected as binders (sucrose is used as a control), and are placed in a mortar and mixed evenly with the ultra-microporous metal-organic framework material Al (fum) powder prepared in Example 1. The total mass of the binder and the powder material is 1g, and the mass percentage of the binder is 2% / 5% (HPC), 2% / 5% (PVA), and 5% / 10% (sucrose), respectively. 2mL of deionized water is added in small amounts and multiple times, and stirred to make it into a paste. After it is half dry, it is extruded into spherical particles with a particle size of 1 to 2mm. The molding material is recorded as Al (fum) @ x% B, where B represents the binder, and x% represents the mass of the binder as a percentage of the total mass of the binder and the metal-organic framework material.

[0064] The surface morphologies of the six prepared molding materials are as follows: Figure 6 As shown, Figure 6Among them, A is Al(fum)@5%HPC, B is Al(fum)@2%HPC, C is Al(fum)@5%PVA, D is Al(fum)@2%PVA, E is Al(fum)@10%sucrose, and F is Al(fum)@5%sucrose. The molding effects of the three results are different. Both HPC and PVA have good molding effects, while sucrose has a poor effect. For example, when HPC is used as a binder and the binder dosage is 5%, the operation is relatively convenient during the molding process. The formed particles have good morphology, smooth surface and are not easy to break. When the binder dosage is reduced to 2%, intact particles can still be formed. When PVA is used as a binder, because PVA is insoluble in water at room temperature, it needs to be dissolved in hot water to make a solution before further use. The operation is slightly more troublesome than HPC. 5% and 2% binder dosages can also eventually form particles with good morphology and smooth surface. When sucrose is used as a binder, due to its weak viscosity, it is difficult to form stable particles when the binder dosage is 5%, and it is very easy to break. When the binder dosage is increased to 10%, the viscosity increases and particles can be formed, but the surface is not smooth enough and has obvious cracks.

[0065] Example 4

[0066] Weigh 980 mg of the ultra-microporous metal-organic framework material Al(fum) powder (not degassed) prepared in Example 1 and 20 mg of hydroxypropyl cellulose (HPC), place them in a mortar and mix them evenly, add 2 mL of deionized water in small amounts and multiple times, stir to make it into a paste, and after it is half dry, squeeze it into spherical particles with a particle size of 1 to 2 mm. After drying, a molded ultra-microporous metal-organic framework material, i.e., Al(fum)@HPC particles with a binder mass fraction of 2%, is obtained, recorded as Al(fum)@2%HPC.

[0067] The thermogravimetric curve of the ultra-microporous metal-organic framework Al(fum)@2%HPC obtained in this example is as follows: Figure 7 As shown, it can be seen that the material still maintains excellent thermal stability after molding.

[0068] The formed ultra-microporous metal-organic framework material Al(fum)@2%HPC was analyzed by X-ray diffraction. The results are as follows: Fig. 9 As shown. Fig. 9 It can be seen that the peak shape of the material formed with 2% HPC as a binder is consistent with the ultra-microporous metal-organic framework powder material, proving that the Al(fum)@2% HPC framework structure remains intact after forming.

[0069] The Al(fum)@2%HPC shaped granular material was placed in a vacuum degassing at 120°C for 24 hours, and the degassing pressure was less than 5μmHg. Then, the single-component static adsorption isotherm of N2 was tested on a Micrometrics ASAP 2460 adsorption instrument at a test temperature of 77K. Test results: The adsorption isotherm of N2 of the shaped ultra-microporous material Al(fum)@2%HPC obtained in this embodiment at 77K is as follows: Fig.10 As shown in A, the N2 adsorption curve of the material after molding is consistent with the adsorption curve of the ultra-microporous metal-organic framework material powder, and the specific surface area remains basically unchanged (Al(fum)@2%HPC:999m 2 / g, Al(fum):1040m 2 / g).

[0070] The single component static adsorption isotherms of SF6, CF4 and N2 were tested on Micrometrics ASAP 2460 adsorption instrument at 298K. The test results are as follows: Fig.12 As shown. The adsorption curve of Al(fum)@2% HPC particles for SF6 is still very steep at low pressure, and the SF6 adsorption at 298K and 10kPa can still maintain 2.67mmol / g. The SF6 adsorption at 273K is slightly higher than that at 298K, and is 3.04mmol / g at 10kPa, which is about 5% lower than that of the powder (3.20mmol / g). The adsorption of CF4 by Al(fum)@2% HPC particles is also reduced. For example, at 100kPa, the CF4 adsorption at 298K is 1.73mmol / g, which is 6.5% lower than that of the powder material. However, the adsorption of N2 by Al(fum)@2% HPC particles is still very low. For example, at 100kPa, the N2 adsorption at 298K is 0.23mmol / g, which is basically unchanged compared with the original powder. It shows that the formed Al(fum)@2% HPC particles still have good SF6 / N2 and SF6 / CF4 separation potential.

[0071] Weigh 200 mg of Al(fum)@2% HPC particles after molding and place them in a conical bottle. Place it in an oscillating incubator at 25°C and 300 rpm and record the mass change of the particles. Fig.11 It shows that the Al(fum)@2% HPC particles after molding have good mechanical properties, and the mass loss is within 0.4% after 24 hours.

[0072] Example 5

[0073] Weigh 950 mg of the ultra-microporous metal-organic framework material Al(fum) powder (not degassed) prepared in Example 1 and 50 mg of hydroxypropyl cellulose (HPC), place them in a mortar and mix them evenly, add 2 mL of deionized water in small amounts and multiple times, stir to make it into a paste, and after it is half dry, squeeze it into spherical particles with a particle size of 1 to 2 mm. After drying, a molded ultra-microporous metal-organic framework material, i.e., Al(fum)@HPC particles with a binder mass fraction of 5%, is obtained, recorded as Al(fum)@5%HPC.

[0074] The thermogravimetric curve of the ultra-microporous material Al(fum)@5%HPC obtained in this example is as follows: Figure 7 As shown, it can be seen that the material still maintains excellent thermal stability after molding.

[0075] X-ray diffraction was used to analyze the material forming ultra-microporous material Al(fum)@5%HPC. The results are as follows: Fig. 9 As shown. Fig. 9 It can be seen that the peak shape of the material formed with 5% HPC as a binder is consistent with that of the powder material, proving that the Al(fum)@5% HPC framework structure remains intact after forming.

[0076] Weigh 200 mg of the formed Al(fum)@5% HPC into a conical flask, place it in an oscillating incubator at 25°C and 300 rpm, and record the mass change of the particles. Fig.11 It can be seen that the Al(fum)@5% HPC particles have good mechanical properties after molding, and the mass loss is within 0.4% after 24 hours.

[0077] Example 6

[0078] Weigh 980 mg of the ultra-microporous metal-organic framework material Al(fum) powder (not degassed) prepared in Example 1 and 20 mg of polyvinyl alcohol (PVA), place them in a mortar and mix them evenly, add 2 mL of deionized water in small amounts and several times, stir to make it into a paste, and after it is half dry, squeeze it into spherical particles with a particle size of 1 to 2 mm. After drying, a molded ultra-microporous metal-organic framework material, i.e., Al(fum)@PVA particles with a binder mass fraction of 2%, is obtained, recorded as Al(fum)@2%PVA.

[0079] The thermogravimetric curve of the ultra-microporous material Al(fum)@2%PVA obtained in this example is as follows: Figure 8 As shown, it can be seen that the material still maintains excellent thermal stability after molding.

[0080] The X-ray diffraction analysis of the molded ultra-microporous material Al(fum)@2%PVA showed the following results: Fig. 9 As shown. Fig. 9 It can be seen that the peak shape of the material after molding with 2% PVA as a binder is consistent with that of the powder material, proving that the Al(fum)@2% PVA framework structure remains intact after molding.

[0081] The Al(fum)@2%PVA shaped particles were placed in a vacuum degassing at 120°C for 24 hours with a degassing pressure lower than 5μmHg. Then, the single component static adsorption isotherm of N2 was tested on a Micrometrics ASAP 2460 adsorption instrument at a test temperature of 77K. The adsorption isotherm of N2 of the shaped ultra-microporous material Al(fum)@2%PVA obtained in this example at 77K is as follows: Fig.10 As shown in B, the N2 adsorption curve of the material after molding is consistent with the adsorption curve of the powder, and the specific surface area remains basically unchanged (Al(fum)@2%PVA:958m 2 / g, Al(fum):1040m 2 / g).

[0082] Weigh 200 mg of the molded Al(fum)@2%PVA into a conical flask, place it in an oscillating incubator at 25°C and 300 rpm, and record the mass change of the particles, such as Fig.11 It can be seen that the Al(fum)@2%PVA particles after molding have good mechanical properties, and the mass loss is within 0.4% after 24 hours.

[0083] Example 7

[0084] Weigh 950 mg of the ultra-microporous metal-organic framework material Al(fum) powder (not degassed) prepared in Example 1 and 50 mg of polyvinyl alcohol (PVA), place them in a mortar and mix them evenly, add 2 mL of deionized water in small amounts and multiple times, stir to make it into a paste, and after it is half dry, squeeze it into spherical particles with a particle size of 1 to 2 mm. After drying, the molded ultra-microporous metal-organic framework material, i.e., Al(fum)@PVA particles with a binder mass fraction of 5%, recorded as Al(fum)@5%PVA, is obtained.

[0085] The thermogravimetric curve of the ultra-microporous material Al(fum)@5%PVA obtained in this example is as follows: Figure 8 As shown, it can be seen that the material still maintains excellent thermal stability after molding.

[0086] X-ray diffraction was used to analyze the material forming ultra-microporous material Al(fum)@5%PVA. The results are as follows: Fig. 9 As shown. Fig. 9It can be seen that the peak shape of the material after molding with 5% PVA as a binder is consistent with that of the powder material, proving that the Al(fum)@5% PVA framework structure remains intact after molding.

[0087] Weigh 200 mg of the molded Al(fum)@5% PVA into a conical flask, place it in an oscillating incubator at 25°C and 300 rpm, and record the mass change of the particles. Fig.11 It can be seen that the Al(fum)@5%PVA particles after molding have good mechanical properties, and the mass loss is within 0.4% after 24 hours.

[0088] Example 8

[0089] The shaped ultra-microporous material Al(fum)@2%HPC obtained in Example 4 is loaded into a 10mm×100mm fixed bed adsorption column, and SF6 / N2 (volume ratio 10:90) mixed gas or SF6 / CF4 (volume ratio 4:96) mixed gas is passed into the adsorption column at a flow rate of 1.3mL / min at 273K or 298K, and high-purity N2 (purity greater than 99.999%) is obtained in the outflowing gas; when SF6 penetrates, the adsorption is stopped, and high-purity SF6 (purity greater than 99.99%) can be obtained by desorption by He gas purging at 40°C for 10h, and the adsorption column can be recycled.

[0090] The penetration curve of the formed ultra-microporous material Al(fum)@2%HPC obtained in this example is as follows Fig.13 As shown, the mixed gas flow rate is 1.3mL / min. It can be seen that the material still maintains excellent dynamic SF6 adsorption after molding. High-purity SF6 (greater than 99.99%) can be obtained by desorption at 40°C and 6.0mL He gas purge conditions for 10 hours. The desorption curve is shown in Fig.14 And the SF6 dynamic adsorption capacity of Al(fum)@2%HPC for SF6 / N2 (volume ratio 10:90) mixed gas at 298K after 4 adsorption-desorption cycles did not decrease significantly (as shown in Figure 2). Fig.15 shown).

[0091] It can be seen from the above examples that the molded ultra-microporous metal-organic framework material prepared by the present invention has a high adsorption capacity for SF6 and good selectivity, and can achieve effective separation of SF6 / N2 or SF6 / CF4.

[0092] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a molded ultra-microporous metal-organic framework material, comprising the following steps: The ultra-microporous metal-organic framework material, a binder and water are mixed and wet granulated to obtain the molded ultra-microporous metal-organic framework material; the binder is one or more of hydroxyethyl cellulose, hydroxypropyl cellulose, polyvinyl alcohol, polyvinyl butyral and kaolin; the ultra-microporous metal-organic framework material has infinitely extended periodic one-dimensional square channels with a pore size of 5.7-6.0 Å; The ultra-microporous metal-organic framework material is prepared by mixing a soluble metal salt, an organic ligand, a base and water through a coordination reaction; the metal ion in the soluble metal salt is Cr 3+ 、Al 3+ 、V 3+ and Fe 3+ One or more of the above; the organic ligand is fumaric acid or a fumaric acid derivative, and the fumaric acid derivative has a structure shown in Formula I: Formula I, In formula I, R1 and R2 are independently selected from H, F, Cl, Br, I or CH3, and R1 and R2 are not H at the same time.

2. The preparation method according to claim 1, characterized in that: The mass of the binder is 0.1-15% of the sum of the mass of the binder and the ultra-microporous metal-organic framework material.

3. The preparation method according to claim 1, characterized in that: The particle size of the molded ultra-microporous metal-organic framework material is 1-2 mm.

4. The preparation method according to claim 1, characterized in that: The alkali is sodium hydroxide; the molar ratio of the metal ions in the organic ligand and the soluble metal salt to the alkali is 1-2:2:4-8.

5. The shaped ultra-microporous metal-organic framework material prepared by the preparation method according to any one of claims 1 to 4.

6. Use of the molded ultra-microporous metal-organic framework material according to claim 5 for selectively adsorbing sulfur hexafluoride from a mixed gas; the mixed gas comprises sulfur hexafluoride and nitrogen or comprises sulfur hexafluoride and carbon tetrafluoride.

7. The use according to claim 6, characterized in that: The volume ratio of sulfur hexafluoride to nitrogen or sulfur hexafluoride to carbon tetrafluoride in the mixed gas is 99:1 to 1:

99.

8. The use according to claim 6 or 7, characterized in that: The adsorption is one or more of fixed bed adsorption, fluidized bed adsorption and moving bed adsorption; the adsorption temperature is -20~60°C and the pressure is 0.5~10 bar.