A water-based epoxy compounded reed straw modified emulsified asphalt and its preparation method and application

Through the modification of water-based epoxy compound reed straw, combined with reed straw fiber and other components, the rut resistance and high-temperature flow resistance of emulsified asphalt is improved, and the problem of poor high and low temperature durability of existing emulsified asphalt is solved. It is suitable for high-grade roads. Asphalt demand.

CN116589866BActive Publication Date: 2024-11-19EAST CHINA UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310674710.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-08
Publication Date
2024-11-19
Estimated Expiration
2043-06-08

AI Technical Summary

Technical Problem

The existing emulsified asphalt has poor resistance to rut and high-temperature flow resistance, and has poor high-temperature durability, which cannot meet the performance requirements of high-grade road asphalt.

Method used

By modifying the reed straw by water-based epoxy compound reed straw, reed straw fibers, polyphosphate, glass fibers, rheology modifiers and epoxy resins, the rheology performance and viscosity of the asphalt are improved and its resistance to rut at high temperatures Deformation and resistance to high temperature flow.

Benefits of technology

It significantly improves the high and low temperature durability of emulsified asphalt, enhances its resistance to rut deformation and high temperature flow under high temperatures, and is suitable for road maintenance processes such as fog seals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116589866B_ABST
    Figure CN116589866B_ABST
Patent Text Reader

Abstract

The present invention relates to a water-based epoxy compounded reed straw modified emulsified asphalt and its preparation method and application, which are mainly used in road pre-maintenance and road surface disease treatment methods. The emulsified asphalt mainly includes the following raw materials: 60 parts by weight of petroleum asphalt, 40 parts by weight of water, 1.2-1.8 parts by weight of reed straw, 0.4 parts by weight of emulsifier A, 0.2 parts by weight of emulsifier B, 0.2 parts by weight of stabilizer, 5-6 parts by weight of epoxy resin emulsion, 2.5-3 parts by weight of liquid epoxy resin curing agent, 2 parts by weight of polyphosphate, 3 parts by weight of glass fiber, and 2 parts by weight of rheology modifier. Compared with the prior art, the emulsified asphalt prepared by the present invention greatly improves the problems of insufficient durability and rutting resistance of asphalt, and at the same time, the low-temperature performance of the emulsified asphalt during modification is also taken into account, which solves the problems of poor rutting resistance and poor low-temperature plasticity when the emulsified asphalt is used as a protective material to the greatest extent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of road asphalt processing, and in particular to a water-based epoxy compounded reed straw modified emulsified asphalt and a preparation method and application thereof. Background Art

[0002] In general, the application of emulsified asphalt in road construction mainly includes two construction methods: spraying and mixing. Common application scenarios of spraying construction mainly include use as penetration oil, tack coat oil and sealing oil. The penetration oil is mainly a thin layer that penetrates the surface in order to make the non-asphalt layer such as semi-rigid base layer and the asphalt layer material combine well during the road paving process. Emulsified asphalt is used in this process because of its good fluidity and permeability; the spraying of tack coat oil is to make the old asphalt layer material and the new asphalt layer material combine well; the use of sealing oil is mainly to fill the gaps between aggregates and isolate the erosion of air and rainwater, thereby extending the service life of the road. Common application methods include fog seal, gravel seal, fine chip seal, etc. In the process of gravel seal and fine chip seal, after spraying emulsified asphalt on the road surface, stones of different particle sizes are spread and rolled to form a thin layer. The development of emulsified asphalt mixing construction technology is more diverse. Common ones include slurry seal, micro-surfacing technology, cold mix asphalt mixture and cold mix asphalt recycling technology. These technologies are often used for pre-maintenance of road asphalt and prevention and treatment of pavement diseases.

[0003] Emulsified asphalt is used as a binder material in construction. When base emulsified asphalt is used and no modifying material is added, the emulsified asphalt will have problems such as poor bonding performance, low material strength, and poor durability after demulsification. At the same time, the demand for high-grade road asphalt in road construction is getting higher and higher, so the requirements for road asphalt performance are also gradually increasing. In order to solve this problem, the modification technology of emulsified asphalt has been developed. The modification of emulsified asphalt can be divided into two categories according to the modification process sequence: 1. First emulsify the base asphalt and then use the modifier to modify it; 2. First modify the hot asphalt and then emulsify it.

[0004] In the Chinese patent with publication number CN114395266A and invention name "A water-based epoxy resin modified emulsified asphalt and its preparation method", an emulsified asphalt is obtained by modifying epoxy resin emulsion, curing agent, liquid rubber and dicarboxylic acid; in the Chinese patent with publication number CN112409806A and invention name "A single-component water-based epoxy SBS composite modified emulsified asphalt", SBS and maleic anhydride are added to the base asphalt in sequence to obtain maleic anhydride / SB S modified asphalt, and then adding polyurethane and epoxy resin emulsion to obtain a one-component water-based epoxy resin / SBS composite modified emulsified asphalt; the Chinese patent with publication number CN114276559A and invention name "A water-based epoxy resin emulsion for pre-curing wear layer of asphalt pavement and its preparation method" discloses an epoxy resin emulsifier prepared from epoxy resin / polyol diglycidyl ether-amine adduct, which improves the toughness of epoxy resin emulsion and its compatibility with cationic emulsified asphalt.

[0005] However, the existing emulsified asphalt has poor anti-rutting and high-temperature flow properties, and poor high and low temperature durability. Therefore, there is an urgent need for an emulsified asphalt that can solve the above problems. Summary of the invention

[0006] The purpose of the present invention is to solve the above problems and to provide a water-based epoxy compounded reed straw modified emulsified asphalt and its preparation method and application. By modifying the emulsified asphalt with water-based epoxy compounded reed straw, the problems of poor rutting resistance and high temperature flow resistance of the existing emulsified asphalt and poor high and low temperature durability can be solved.

[0007] During the process of conception, the applicant believed that reed straw is rich in plant fiber, which can improve the toughness of asphalt mixture and enhance the ductility of asphalt at low temperatures; epoxy resin, glass fiber, rheology modifier and polyphosphate can comprehensively improve the rheological properties of asphalt, greatly enhance the rigidity of asphalt, increase the viscosity of asphalt, etc., and can enhance the ability of asphalt to resist rutting deformation and high-temperature flow at high temperatures. After compounding these ingredients, the asphalt is modified, and the durability of asphalt at high and low temperatures is comprehensively improved.

[0008] The purpose of the present invention is achieved through the following technical solutions:

[0009] The first object of the present invention is to provide a method for preparing waterborne epoxy composite reed straw modified emulsified asphalt, the preparation method comprising the following steps:

[0010] S1: Heat the petroleum asphalt to a fluid state and pour it into the asphalt tank of the colloid mill, maintain the temperature between 140℃ and 150℃, adjust the asphalt tank reversing valve to the circulation position, then start the asphalt pump and set the asphalt tank flow rate for standby use;

[0011] S2: Add reed straw, polyphosphate, glass fiber, and rheology modifier to the asphalt tank in step S1 in sequence, turn on the stirring device, stir and circulate until the mixture is uniformly mixed, and keep the temperature at 140°C to 150°C;

[0012] S3, preparing an emulsifier mixture in an emulsion tank of a colloid mill, wherein the emulsifier mixture includes water, emulsifier A, emulsifier B, and a stabilizer, turning on the emulsion tank for heating and simultaneously turning on a stirring device, adjusting the reversing valve of the emulsion tank to a circulation position, then turning on an emulsion pump and setting the flow rate of the emulsion tank for standby use;

[0013] S4: The reversing valves of the emulsion tank and the asphalt tank are adjusted to the discharge position at the same time, and the colloid mill is started to perform high-speed shearing, and the discharge of the colloid mill is cooled to obtain a first mixture;

[0014] S5: adding epoxy resin emulsion and epoxy curing agent to the first mixture in S4 respectively, and stirring them thoroughly to obtain the water-based epoxy composite reed straw modified emulsified asphalt.

[0015] Furthermore, the specific process of step S3 is as follows:

[0016] S31: Add water to the emulsion tank of the colloid mill, set the heating temperature to 60°C, start the heating of the emulsion tank and start the stirring device at the same time, adjust the reversing valve of the emulsion tank to the circulation position, then start the emulsion pump and set the flow rate of the emulsion tank for standby use;

[0017] S32: When the temperature of the emulsion tank in step S31 is stabilized at 60°C, emulsifier A, emulsifier B and stabilizer are added in sequence, and stirred sufficiently to completely dissolve them. Then, the pH value of the liquid in the emulsion tank is maintained at 2.0-2.5 by acid adjustment to prepare an emulsifier mixture for use.

[0018] Furthermore, the emulsifier A described in step S32 is a fast-breaking cationic solid emulsifier; the emulsifier B described in step S32 is a non-ionic emulsifier; the stabilizer described in step S32 is guar gum; and the acid used in the acid adjustment described in step S32 is concentrated hydrochloric acid.

[0019] Furthermore, the petroleum asphalt described in step S1 is one of 70# asphalt or 50# asphalt.

[0020] Furthermore, the reed straw described in step S2 is the reed straw obtained by acid washing, alkali washing, water washing and drying of the reed straw to be treated.

[0021] Furthermore, the epoxy resin described in step S5 is a milky white liquid with good fluidity at room temperature.

[0022] Furthermore, the epoxy curing agent described in step S5 is a light yellow liquid with good fluidity at room temperature.

[0023] Furthermore, the high-speed shearing rate in step S4 is 4000 rpm.

[0024] Furthermore, the weight ratio of the epoxy resin emulsion and the epoxy curing agent in step S5 is epoxy resin emulsion:epoxy curing agent=2:1.

[0025] Furthermore, the flow rate ratio of the asphalt tank to the emulsion tank in steps S1 and S3 is 3:2.

[0026] Furthermore, the above preparation method improves the anti-rutting and high-temperature flow properties of the emulsified asphalt after curing, and improves its high-temperature durability and low-temperature durability. The prepared emulsified asphalt has excellent and balanced high and low-temperature performance.

[0027] The second object of the present invention is to provide a water-based epoxy composite reed straw modified emulsified asphalt, which is prepared by the above-mentioned preparation method, and the emulsified asphalt comprises the following components in parts by weight: 60 parts of petroleum asphalt; 40 parts of water; 0.4 parts of emulsifier A; 0.2 parts of emulsifier B; 0.2 parts of stabilizer; reed straw (1.2-1.8) parts; epoxy resin emulsion (5-6) parts; epoxy curing agent (2.5-3) parts; polyphosphate 2 parts; glass fiber 3 parts; rheology modifier 2 parts.

[0028] Optionally, the emulsified asphalt includes the following components in parts by weight: 60 parts of petroleum asphalt; 40 parts of water; 0.4 parts of emulsifier A; 0.2 parts of emulsifier B; 0.2 parts of stabilizer; 1.2 parts of reed straw; 5 parts of epoxy resin emulsion; 2.5 parts of epoxy curing agent; 2 parts of polyphosphate; 3 parts of glass fiber; and 2 parts of rheology modifier.

[0029] Optionally, the emulsified asphalt includes the following components in parts by weight: 60 parts of petroleum asphalt; 40 parts of water; 0.4 parts of emulsifier A; 0.2 parts of emulsifier B; 0.2 parts of stabilizer; 1.8 parts of reed straw; 6 parts of epoxy resin emulsion; 3 parts of epoxy curing agent; 2 parts of polyphosphate; 3 parts of glass fiber; and 2 parts of rheology modifier.

[0030] The third object of the present invention is to provide an application of an aqueous epoxy compounded reed straw modified emulsified asphalt, which can be applied to road maintenance processes such as fog sealing, and can be used in road pre-maintenance and road surface disease treatment methods.

[0031] Compared with the prior art, the present invention has the following advantages:

[0032] The preparation method of the water-based epoxy composite reed straw modified emulsified asphalt of the present invention improves the anti-rutting and high-temperature flow properties of the emulsified asphalt after curing, and improves its high-temperature durability and low-temperature durability. The prepared emulsified asphalt has excellent and balanced high and low-temperature performance and can be applied to road maintenance processes such as fog sealing layers. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is a diagram showing the stone falling off after the brushing and abrasion test in Example 1.

[0034] Figure 2 This is a diagram of the stone falling off after the sweeping and abrasion test in Comparative Example 1.

[0035] Figure 3 This is a diagram of the stone falling off after the sweeping and abrasion test in Example 2.

[0036] Figure 4 This is a diagram of the stone falling off after the sweeping and abrasion test in Comparative Example 2.

[0037] Figure 5 This is a diagram showing the stone falling off after the low-temperature flat plate impact test in Example 1.

[0038] Figure 6 This is a diagram of the stone falling off after the low-temperature flat plate impact test in Comparative Example 1.

[0039] Figure 7 This is a diagram of the stone falling off after the low-temperature flat plate impact test in Example 2.

[0040] Figure 8 This is a diagram of the stone falling off after the low-temperature flat plate impact test in Comparative Example 2. DETAILED DESCRIPTION

[0041] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0042] The specific steps of the preparation method of the water-based epoxy composite reed straw modified emulsified asphalt are:

[0043] S1: Heat the petroleum asphalt to a fluid state and pour it into the asphalt tank of the colloid mill, maintain the temperature between 140℃ and 150℃, adjust the asphalt tank reversing valve to the circulation position, then start the asphalt pump and set the asphalt tank flow rate for standby use;

[0044] S2: Add reed straw, polyphosphate, glass fiber, and rheology modifier to the asphalt tank in step S1 in sequence, turn on the stirring device, stir and circulate until the mixture is uniformly mixed, and keep the temperature at about 140°C to 150°C;

[0045] S3: Add water to the emulsion tank of the colloid mill, set the heating temperature to 60°C, turn on the heating of the emulsion tank and the stirring device at the same time, adjust the reversing valve of the emulsion tank to the circulation position, then turn on the emulsion pump and set the flow rate of the emulsion tank for standby use;

[0046] S4: When the temperature of the emulsion tank in step S3 is stabilized at about 60°C, emulsifier A, emulsifier B, and stabilizer are added in sequence, and stirred sufficiently to completely dissolve them, and then the pH value of the liquid in the emulsion tank is maintained at about 2.0 to 2.5 by acid adjustment, and then set aside;

[0047] S5: The reversing valves of the emulsion tank and the asphalt tank are adjusted to the discharge position at the same time, and the colloid mill is started to perform high-speed shearing, and the discharge of the colloid mill is cooled to obtain a first mixture;

[0048] S6: Add epoxy resin emulsion and epoxy curing agent to the first mixture in S5 in a ratio of epoxy resin emulsion: epoxy curing agent = 2:1, and stir well to obtain the water-based epoxy composite reed straw modified emulsified asphalt.

[0049] Any features such as preparation methods, materials, structures or composition ratios that are not clearly described in this technical solution shall be deemed as common technical features disclosed in the prior art.

[0050] In the following embodiments of the present invention, petroleum asphalt is 70# asphalt produced by Ningbo SK Baoying Asphalt Storage Co., Ltd.; emulsifier A is a fast-cracking cationic solid emulsifier, model 4819, produced by Akzo Nobel; emulsifier B is a non-ionic emulsifier, model Berol 611, produced by Akzo Nobel; the stabilizer is guar gum, produced by Nantong Guangrun New Material Technology Co., Ltd.; the reed straw is the reed straw obtained by acid washing, alkali washing, and subsequent water washing and drying; the epoxy resin emulsion model is 0916A-50W, produced by Nantong Xingchen Synthetic Materials Co., Ltd.; the epoxy curing agent model is 0916B-55W, produced by Nantong Xingchen Synthetic Materials Co., Ltd.; the polyphosphate model is P815555, produced by Maclean; the glass fiber model is BLXW01, produced by Changzhou Bochao Engineering Materials Co., Ltd.; the rheology modifier model is NY-9421, produced by Guangdong Nuoyi Chemical Co., Ltd., and the remaining raw materials are commercially available.

[0051] Example 1

[0052] This embodiment provides a water-based epoxy compounded reed straw modified emulsified asphalt, including the following components by weight:

[0053] 70# asphalt: 1200g; water 800g, emulsifier A 8g, emulsifier B 4g, stabilizer 4g; reed straw 24g, polyphosphate 40g, glass fiber 60g, rheology modifier 40g; epoxy resin emulsion 100g, epoxy curing agent 50g.

[0054] The preparation method of the above-mentioned water-based epoxy composite reed straw modified emulsified asphalt comprises the following steps:

[0055] S1: Heat 70# asphalt to a fluid state and pour it into the asphalt tank of the colloid mill, maintain the temperature between 140℃ and 150℃, adjust the asphalt tank reversing valve to the circulation position, then start the asphalt pump and set the asphalt tank flow rate for standby use;

[0056] S2: Add reed straw, polyphosphate, glass fiber, and rheology modifier to the asphalt tank in step S1 in sequence, turn on the stirring device, stir and circulate until the mixture is uniformly mixed, and keep the temperature at about 140°C to 150°C;

[0057] S3: Add water to the emulsion tank of the colloid mill, set the heating temperature to 60°C, turn on the heating of the emulsion tank and the stirring device at the same time, adjust the reversing valve of the emulsion tank to the circulation position, then turn on the emulsion pump and set the flow rate of the emulsion tank for standby use;

[0058] S4: When the temperature of the emulsion tank in step S3 is stabilized at about 60°C, emulsifier A, emulsifier B, and stabilizer are added in sequence, and stirred sufficiently to completely dissolve them, and then the pH value of the liquid in the emulsion tank is maintained at about 2.0 to 2.5 by acid adjustment, and then set aside;

[0059] S5: The reversing valves of the emulsion tank and the asphalt tank are adjusted to the discharge position at the same time, and the colloid mill is started to perform high-speed shearing, and the discharge of the colloid mill is cooled to obtain a first mixture;

[0060] S6: adding epoxy resin emulsion and epoxy curing agent to the first mixture in S5 respectively, and stirring them thoroughly to obtain the water-based epoxy composite reed straw modified emulsified asphalt.

[0061] The water-based epoxy compounded reed straw modified emulsified asphalt in this embodiment was subjected to high temperature sweeping durability test and low temperature impact durability test respectively. The relevant results are as follows: Figure 1 and Figure 5 shown.

[0062] Example 2

[0063] This embodiment provides a water-based epoxy compounded reed straw modified emulsified asphalt, including the following components by weight:

[0064] 50# asphalt: 1200g; water 800g, emulsifier A 8g, emulsifier B 4g, stabilizer 4g; reed straw 36g, polyphosphate 40g, glass fiber 60g, rheology modifier 40g epoxy resin emulsion 120g, epoxy curing agent 60g.

[0065] The preparation method of the above-mentioned water-based epoxy composite reed straw modified emulsified asphalt comprises the following steps:

[0066] S1: Heat 50# asphalt to a fluid state and pour it into the asphalt tank of the colloid mill, maintain the temperature between 140℃ and 150℃, adjust the asphalt tank reversing valve to the circulation position, then start the asphalt pump and set the asphalt tank flow rate for standby use;

[0067] S2: Add reed straw, polyphosphate, glass fiber, and rheology modifier to the asphalt tank in step S1 in sequence, turn on the stirring device, stir and circulate until the mixture is uniformly mixed, and keep the temperature at about 140°C to 150°C;

[0068] S3: Add water to the emulsion tank of the colloid mill, set the heating temperature to 60°C, turn on the heating of the emulsion tank and the stirring device at the same time, adjust the reversing valve of the emulsion tank to the circulation position, then turn on the emulsion pump and set the flow rate of the emulsion tank for standby use;

[0069] S4: When the temperature of the emulsion tank in step S3 is stabilized at about 60°C, emulsifier A, emulsifier B, and stabilizer are added in sequence, and stirred sufficiently to completely dissolve them, and then the pH value of the liquid in the emulsion tank is maintained at about 2.0 to 2.5 by acid adjustment, and then set aside;

[0070] S5: The reversing valves of the emulsion tank and the asphalt tank are adjusted to the discharge position at the same time, and the colloid mill is started to perform high-speed shearing, and the discharge of the colloid mill is cooled to obtain a first mixture;

[0071] S6: adding epoxy resin emulsion and epoxy curing agent to the first mixture in S5 respectively, and stirring them thoroughly to obtain the water-based epoxy composite reed straw modified emulsified asphalt.

[0072] The water-based epoxy compounded reed straw modified emulsified asphalt in this embodiment was subjected to high temperature sweeping durability test and low temperature impact durability test respectively. The relevant results are as follows: Figure 3 and Figure 7 shown.

[0073] Comparative Example 1

[0074] This comparative example provides an emulsified 70# asphalt, comprising the following components by weight:

[0075] 70# asphalt: 1200g; water 800g, emulsifier A 8g, emulsifier B 4g, stabilizer 4g.

[0076] The preparation method of the above-mentioned emulsified 70# asphalt comprises the following steps:

[0077] S1: Heat 70# asphalt to a fluid state and pour it into the asphalt tank of the colloid mill, maintain the temperature between 140℃ and 150℃, adjust the asphalt tank reversing valve to the circulation position, then start the asphalt pump and set the asphalt tank flow rate to 135 for standby use;

[0078] S2: Turn on the asphalt tank stirring device, stir and circulate it fully, and keep the temperature at about 140℃~150℃;

[0079] S3: Add water to the emulsion tank of the colloid mill, set the heating temperature to 60°C, turn on the heating of the emulsion tank and the stirring device at the same time, adjust the reversing valve of the emulsion tank to the circulation position, then turn on the emulsion pump and set the flow rate of the emulsion tank to 90, and set it for standby;

[0080] S4: When the temperature of the emulsion tank in step S3 is stabilized at about 60°C, emulsifier A, emulsifier B, and stabilizer are added in sequence, and stirred sufficiently to completely dissolve them, and then the pH value of the liquid in the emulsion tank is maintained at about 2.0 to 2.5 by acid adjustment, and then set aside;

[0081] S5: The reversing valves of the emulsion tank and the asphalt tank are adjusted to the discharging position at the same time, and the colloid mill is turned on for high-speed shearing. After the discharging material of the colloid mill is cooled, the emulsified 70# asphalt is obtained.

[0082] The emulsified 70# asphalt in this comparative example was subjected to high temperature sweeping durability test and low temperature impact durability test respectively. The relevant results are as follows Figure 2 and Figure 6 shown.

[0083] Comparative Example 2

[0084] This comparative example provides an emulsified 50# asphalt, comprising the following components by weight:

[0085] 70# asphalt: 1200g; water 800g, emulsifier A 8g, emulsifier B 4g, stabilizer 4g.

[0086] The preparation method of the above-mentioned emulsified 50# asphalt comprises the following steps:

[0087] S1: Heat 50# asphalt to a fluid state and pour it into the asphalt tank of the colloid mill, maintain the temperature between 140℃ and 150℃, adjust the asphalt tank reversing valve to the circulation position, then start the asphalt pump and set the asphalt tank flow rate to 135 for standby use;

[0088] S2: Turn on the asphalt tank stirring device, stir and circulate it fully, and keep the temperature at about 140℃~150℃;

[0089] S3: Add water to the emulsion tank of the colloid mill, set the heating temperature to 60°C, turn on the heating of the emulsion tank and the stirring device at the same time, adjust the reversing valve of the emulsion tank to the circulation position, then turn on the emulsion pump and set the flow rate of the emulsion tank to 90, and set it for standby;

[0090] S4: When the temperature of the emulsion tank in step S3 is stabilized at about 60°C, emulsifier A, emulsifier B, and stabilizer are added in sequence, and stirred sufficiently to completely dissolve them, and then the pH value of the liquid in the emulsion tank is maintained at about 2.0 to 2.5 by acid adjustment, and then set aside;

[0091] S5: The reversing valves of the emulsion tank and the asphalt tank are adjusted to the discharging position at the same time, and the colloid mill is turned on for high-speed shearing. After the discharging material of the colloid mill is cooled, the emulsified 50# asphalt is obtained.

[0092] The emulsified base asphalt in this comparative example was subjected to high temperature sweeping durability test and low temperature impact durability test respectively. The relevant results are as follows Figure 4 and Figure 8 shown.

[0093] The products obtained from the above-mentioned Examples 1 to 2 and Comparative Examples 1 to 2 were subjected to emulsified asphalt sweeping and abrasion test, emulsified asphalt Vialit plate impact test and emulsified asphalt storage stability test. The emulsified asphalt sweeping and abrasion test was designed based on the test method ASTM American Society for Testing and Materials standard D7000-11, and the experimental condition was a 60°C water bath; in the experimental method T 0660-200, hot asphalt was used to test the low-temperature adhesion between asphalt and aggregate, and a plate impact test suitable for emulsified asphalt was designed based on this experimental method, and the experimental condition was a 15°C water bath; the storage stability test was conducted according to the T 0655-1993 method in JTG E20-2011 "Test Procedures for Asphalt and Mixtures in Highway Engineering". The test results of Examples 1 to 2 and Comparative Examples 1 to 2 are shown in Table 1; for comparison Figure 1 and Figure 2 ,contrast Figure 3 and Figure 4 It can be seen that the water-based epoxy modified emulsified asphalt provided by the present invention does not cause obvious stone shedding after high-temperature sweeping; Figure 5 and Figure 6 ,contrast Figure 7 and Figure 8It can also be seen that the water-based epoxy modified emulsified asphalt provided by the present invention also has a lower stone drop rate after the low-temperature impact test. The experimental results show that the water-based epoxy composite reed straw modified emulsified asphalt and the preparation method thereof provided by the present invention have obvious improvement effects on improving the high-temperature sweeping test and low-temperature impact evaluation of the emulsified asphalt compared with the original emulsified asphalt, have good storage stability, and have a more significant improvement effect.

[0094] Table 1 Experimental results.

[0095] Brush wear loss rate / % Flat plate impact loss rate / % Storage stability (5 days) / % Example 1 33.9 80.5 2.9 Example 2 22.9 81.5 3.5 Comparative Example 1 48.5 98.0 2.2 Comparative Example 2 47.7 98.0 3.3

[0096] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A method for preparing water-based epoxy composite reed straw modified emulsified asphalt, It is characterized in that The preparation method comprises the following steps: S1: Heat the petroleum asphalt to a fluid state and pour it into the asphalt tank of the colloid mill, maintain the temperature between 140℃ and 150℃, adjust the asphalt tank reversing valve to the circulation position, then start the asphalt pump and set the asphalt tank flow rate for standby use; S2: Add reed straw, polyphosphate, glass fiber, and rheology modifier to the asphalt tank in step S1 in sequence, turn on the stirring device, stir and circulate until the mixture is uniformly mixed, and keep the temperature at 140°C to 150°C; S3, preparing an emulsifier mixture in an emulsion tank of a colloid mill, wherein the emulsifier mixture includes water, emulsifier A, emulsifier B, and a stabilizer, turning on the emulsion tank for heating and simultaneously turning on a stirring device, adjusting the reversing valve of the emulsion tank to a circulation position, then turning on an emulsion pump and setting the flow rate of the emulsion tank for standby use; The specific process of step S3 is as follows: S31: Add water to the emulsion tank of the colloid mill, set the heating temperature to 60°C, start the heating of the emulsion tank and start the stirring device at the same time, adjust the reversing valve of the emulsion tank to the circulation position, then start the emulsion pump and set the flow rate of the emulsion tank for standby use; S32: When the temperature of the emulsion tank in step S31 is stabilized at 60°C, emulsifier A, emulsifier B, and stabilizer are added in sequence, and stirred sufficiently to be completely dissolved, and then the pH value of the liquid in the emulsion tank is maintained at 2.0-2.5 by acid adjustment to prepare an emulsifier mixture for standby use; The emulsifier A described in step S32 is a fast-breaking cationic solid emulsifier; The emulsifier B described in step S32 is a non-ionic emulsifier; The stabilizer described in step S32 is guar gum; The acid used in the acid adjustment in step S32 is concentrated hydrochloric acid; S4: The reversing valves of the emulsion tank and the asphalt tank are adjusted to the discharge position at the same time, and the colloid mill is started to perform high-speed shearing, and the discharge of the colloid mill is cooled to obtain a first mixture; S5: adding epoxy resin emulsion and epoxy curing agent to the first mixture in S4 respectively, and stirring them thoroughly to obtain the water-based epoxy composite reed straw modified emulsified asphalt; The flow rate ratio of the asphalt tank to the emulsion tank in steps S1 and S3 is 3:2; The emulsified asphalt comprises the following components in parts by weight: 60 parts of petroleum asphalt; 40 parts water; Emulsifier A 0.4 part; Emulsifier B 0.2 part; 0.2 parts of stabilizer; Reed straw 1.2-1.8 parts; 5-6 parts of epoxy resin emulsion; Epoxy curing agent 2.5~3 parts; 2 parts of polyphosphate; 3 parts of glass fiber; 2 parts of rheology modifier.

2. A method for preparing a water-based epoxy composite reed straw modified emulsified asphalt according to claim 1, It is characterized in that The petroleum asphalt described in step S1 is one of 70# asphalt or 50# asphalt.

3. A method for preparing a water-based epoxy composite reed straw modified emulsified asphalt according to claim 1, It is characterized in that The reed straw described in step S2 is the reed straw obtained by acid washing, alkali washing, water washing and drying of the reed straw to be treated.

4. A method for preparing a water-based epoxy composite reed straw modified emulsified asphalt according to claim 1, It is characterized in that The rate of the high-speed shearing in step S4 is 4000 rpm.

5. A method for preparing a water-based epoxy composite reed straw modified emulsified asphalt according to claim 1, It is characterized in that The weight ratio of the epoxy resin emulsion to the epoxy curing agent in step S5 is epoxy resin emulsion:epoxy curing agent=2:

1.

6. A water-based epoxy composite reed straw modified emulsified asphalt prepared by the preparation method as described in any one of claims 1 to 5.

7. An application of water-based epoxy composite reed straw modified emulsified asphalt prepared by the preparation method according to any one of claims 1 to 5, It is characterized in that The water-based epoxy compounded reed straw modified emulsified asphalt is used in a road maintenance process.