A high-solid content, high-viscosity and high-elasticity modified emulsified asphalt and preparation method thereof

By using SBS or SBR modifier and warm mixing agent, combined with the emulsification method of high-speed shear instrument and colloid mill, the problems of low solid content and poor viscosity of high-viscosity modified emulsified asphalt are solved, and high solid content and high viscosity are achieved. The preparation of modified emulsified asphalt improves the performance and application prospects of recycled asphalt mixtures.

CN116622249BActive Publication Date: 2024-10-15WUHAN INST OF TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310611130.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-29
Publication Date
2024-10-15
Estimated Expiration
2043-05-29

AI Technical Summary

Technical Problem

The existing high-viscosity modified emulsified asphalt has low solid content, which results in excessive voids in the recycled asphalt mixture and affects the mechanical properties; while the high-solid content emulsified asphalt has poor viscosity properties, making it difficult to achieve good cementing effects and the cost of the modifier. High, the preparation process is complex, which limits its application.

Method used

Use cheap SBS or SBR as the modifier, adjust the viscosity through warm mixing agent, and combine the emulsification method of high-speed shear instrument and colloid mill to prepare high-solid content, high-viscosity and high-elastic modified emulsified asphalt, add stabilizers and Co-emulsifier to improve emulsification success rate and storage stability.

Benefits of technology

It achieves both high solid content and high viscosity, improves the mechanical properties and cohesion of recycled asphalt mixture, reduces production costs, enhances storage stability, and expands application fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004252417300000071
    Figure BDA0004252417300000071
Patent Text Reader

Abstract

The present invention belongs to the technical field of road engineering materials, and discloses a high-solid content, high-viscosity and high-elastic modified emulsified asphalt and a preparation method thereof. The high-solid content, high-viscosity and high-elastic modified emulsified asphalt includes the following components by mass: 100 parts of matrix asphalt, 6-10 parts of modifier, 2-4 parts of elasticizer, 0.5-1.5 parts of plasticizer, 0.5-1.5 parts of stabilizer, 1.5-5 parts of emulsifier, 2-8 parts of warm mix agent, 0.1-0.3 parts of co-emulsifier, 0.1-0.2 parts of pH regulator, and 40-75 parts of water. The present invention uses cheap SBS or SBR as a modifier, adjusts the viscosity of the modified asphalt by a warm mix agent, and adds a certain amount of stabilizer, and then combines two emulsification methods to make the modified asphalt emulsified smoothly, and finally obtains a modified emulsified asphalt with both high solid content and high viscosity and high elasticity, which has broad application prospects in the fields of binder, tack coat oil and slurry seal.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of road engineering materials, and specifically relates to a high-solid content, high-viscosity and high-elasticity modified emulsified asphalt and a preparation method thereof. Background Art

[0002] Emulsified asphalt is first melted asphalt with an emulsifier to reduce the surface tension of water, and then the asphalt and water are dispersed into small particles through the mechanical shear force of a high-speed shearing instrument or a colloid mill to form a water-in-oil or oil-in-water liquid asphalt. Emulsified asphalt is mainly divided into two categories: spraying type and mixing type. Spraying emulsified asphalt can be used for penetration oil, tack oil and lower seal layer, while mixing emulsified asphalt is mainly used for slurry seal, micro-surface treatment and cold mix asphalt mixture. For mixing emulsified asphalt, if the viscosity is insufficient, it will lead to poor adhesion between asphalt and aggregate or road surface, which will cause a series of diseases. If the solid content is insufficient, it will lead to excessive internal voids in the asphalt mixture due to water dispersion after demulsification, affecting its mechanical properties and road performance. Therefore, the preparation of high-solid content, high-viscosity and high-elasticity modified emulsified asphalt will have great practical significance in the field of road engineering.

[0003] The solid content of high-viscosity modified emulsified asphalt on the market is generally less than 50%. When it is used as a binder for recycled asphalt mixture (RAP), a large amount of water needs to evaporate after demulsification, which will cause excessive voids in the recycled asphalt mixture, affecting its mechanical properties and road performance. However, the viscosity performance of ordinary high-solid emulsified asphalt is not good. When it is used as a binder for RAP, it cannot provide sufficient cohesion, making it difficult to achieve good performance of the recycled asphalt mixture. Its performance can only be increased by adding cement and polymer binders, but the addition of such binders often reduces the low-temperature performance of the recycled asphalt mixture. It can be seen that the current technical level is difficult to take into account both high solid content and high viscosity.

[0004] In addition, the preparation of high-viscosity and high-elasticity modified emulsified asphalt is also restricted by many factors. First, the cost of modifiers is relatively high. Currently, there are mainly several types of modifiers, such as thermoplastic elastomers, fibers, and nanomaterials. Tafpack-Super (TPS) is the most widely used. The asphalt prepared by it has excellent performance, but its cost is high and it cannot be used on a large scale. Second, for the preparation process of first modification and then emulsification, the viscosity of the modified asphalt is high, which makes subsequent emulsification difficult, affecting the performance of the final modified emulsified asphalt. The above reasons limit the application of high-viscosity and high-elasticity modified emulsified asphalt, which is also a problem that needs to be solved urgently in the industry. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a high-solid content, high-viscosity and high-elastic modified emulsified asphalt and a preparation method thereof in view of the deficiencies in the prior art. Inexpensive SBS or SBR is used as a modifier, the viscosity of the modified asphalt is adjusted by a warm mix agent, and a certain amount of stabilizer is added. The two emulsification methods are combined to emulsify the modified asphalt smoothly, and finally a modified emulsified asphalt with high solid content, high viscosity and high elasticity is obtained.

[0006] In order to solve the technical problem proposed by the present invention, on the one hand, the present invention provides a high-solid content, high-viscosity and high-elastic modified emulsified asphalt, including the following components in parts by weight: 100 parts of base asphalt, 6-10 parts of modifier, 2-4 parts of elasticizer, 0.5-1.5 parts of plasticizer, 0.5-1.5 parts of stabilizer, 1.5-5 parts of emulsifier, 2-8 parts of warm mix agent, 0.1-0.3 parts of co-emulsifier, 0.1-0.2 parts of pH adjuster, and 40-70 parts of water.

[0007] In the above scheme, the base asphalt is one of 50#, 70#, and 90# road petroleum asphalt.

[0008] In the above scheme, the modifier is SBS (styrene-butadiene-styrene block copolymer) or SBR (polystyrene butadiene copolymer).

[0009] Furthermore, the SBS is star-shaped or linear.

[0010] Furthermore, the SBR is emulsion-polymerized SBR latex or emulsion-polymerized SBR powder.

[0011] Furthermore, the solid content of the emulsion-polymerized SBR latex is 60-90%.

[0012] In the above scheme, the elasticizing agent is rubber powder, which is a black powdery solid processed from waste tires.

[0013] In the above scheme, the plasticizer is one of dioctyl phthalate (DOP) and dibutyl phthalate (DBP).

[0014] In the above scheme, the stabilizer is furfural oil with a purity greater than 80%.

[0015] In the above scheme, the emulsifier is a slow-cracking and fast-setting cationic asphalt emulsifier.

[0016] In the above scheme, the warm mix agent is Sasobite.

[0017] In the above scheme, the auxiliary emulsifier is anhydrous calcium chloride with a purity greater than 95%.

[0018] In the above scheme, the pH regulator is hydrochloric acid with a concentration greater than 38%.

[0019] In the above scheme, the solid content of the high-solid-content, high-viscosity and high-elasticity modified emulsified asphalt is 60-75%.

[0020] Another aspect of the present invention provides a method for preparing a high-solid content, high-viscosity and high-elastic modified emulsified asphalt, comprising the following steps:

[0021] 1) Preparation of modified asphalt: After heating the base asphalt to a first temperature, add a modifier and an elasticizer to perform a primary swelling, start a high-speed shearing instrument to stir and heat at a first speed, when the temperature rises to a second temperature, increase the speed to a second speed to perform a primary shearing, then add a plasticizer and a stabilizer to perform a secondary shearing, stop shearing, and keep warm for a secondary swelling to obtain a modified asphalt;

[0022] 2) preparing soap solution: heating water, adding emulsifier and co-emulsifier in sequence and stirring evenly, and then adjusting the pH with a pH adjuster to obtain soap solution;

[0023] 3) Preparation of high-solid content, high-viscosity and high-elastic modified emulsified asphalt: Start the high-speed shear instrument to stir the soap solution at three-stage speed, then increase the speed to four-stage speed, add the mixture of modified asphalt and warm mix agent into the soap solution for shearing, and quickly transfer it to the preheated colloid mill for grinding after shearing to obtain high-solid content, high-viscosity and high-elastic modified emulsified asphalt.

[0024] In the above scheme, the temperature of the first stage is 140-160°C, and the temperature of the second stage is 175-200°C.

[0025] In the above scheme, the first stage speed is 2000-3000r / min, and the second stage speed is 7000-9000r / min.

[0026] In the above scheme, the primary shearing time is 30-60 minutes, and the secondary shearing time is 15-30 minutes.

[0027] In the above scheme, the time of the first swelling is 10-20 minutes; the temperature of the second swelling is 170-190° C., and the time is 2-3 hours.

[0028] In the above scheme, the heating temperature of the water is 60-70° C., and the pH of the soap solution is 1-2.

[0029] In the above scheme, the three-stage rotation speed is 1000-2000r / min, and the time for stirring the soap solution is 30-60s.

[0030] In the above scheme, the four-stage rotation speed is 7000-8500r / min, and the shearing time after the mixture of modified asphalt and warm mix agent is added is 3-4min.

[0031] In the above scheme, the preheating temperature of the colloid mill is 50-70°C, the grinding speed is 2000-6500r / min, and the grinding time is 30-40s.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] 1) The present invention mainly utilizes traditional modifiers such as SBS or SBR with high dosage to increase the viscosity of modified asphalt. The performance of such modifiers is similar to that of TPS but their price is much lower than that of TPS. However, the compatibility of SBS and SBR with asphalt is poor, making it difficult to disperse them evenly in asphalt, which affects the storage stability of asphalt. Therefore, the present invention adds oils rich in aromatic components to improve the performance, which can not only achieve the preparation of high-solid content, high-viscosity and high-elasticity asphalt at low cost, but also meet the requirements of storage stability.

[0034] 2) The present invention adjusts the viscosity of the modified asphalt by a warm mix agent so that the modified asphalt can be emulsified smoothly, and adds a stabilizer to further improve the success rate of emulsification. The present invention changes the previous emulsification method of using only a high-speed shear instrument or only a colloid mill for emulsification, and combines the two emulsification methods, first pre-emulsification with a high-speed shear instrument and then emulsification with a colloid mill, which can not only improve the success rate of emulsification, but also reduce the particle size of the emulsified asphalt and reduce the risk of colloid mill being blocked, thereby obtaining a high-solid content, high-viscosity and high-elastic emulsified asphalt with good storage stability, which has broad application prospects in the fields of binders, tack coat oils and slurry seals. DETAILED DESCRIPTION

[0035] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.

[0036] In the following examples, the elasticizer used is rubber powder, the stabilizer used is furfural oil with a purity greater than 80%, the emulsifier used is a slow-cracking and fast-setting cationic asphalt emulsifier provided by Shengquan Company, whose model is SQBIO A6, and the warm mix agent used is Sasobite; the auxiliary emulsifier used is anhydrous calcium chloride with a purity greater than 95%, and the pH regulator used is hydrochloric acid with a concentration of 40%.

[0037] Example 1

[0038] A high-solid content, high-viscosity and high-elastic modified emulsified asphalt comprises the following components in parts by mass: 100 parts of 70# road petroleum asphalt, 6 parts of linear SBS (monomer ratio S / B is 3 / 7), 2.5 parts of rubber powder, 1 part of DOP, 0.5 parts of furfural oil, 2 parts of emulsifier, 4 parts of warm mix agent, 0.1 parts of anhydrous calcium chloride, 0.1 parts of hydrochloric acid and 60 parts of deionized water; the designed solid content is 60%.

[0039] The preparation method of the high-solid content, high-viscosity and high-elastic modified emulsified asphalt comprises the following steps:

[0040] 1) Preparation of modified asphalt: After heating 70# road petroleum asphalt to 140°C, add linear SBS and rubber powder to swell for 10 minutes, start the high-speed shearing instrument and stir at a speed of 2000r / min and heat up. When the temperature rises to 175°C, increase the speed to 7000r / min and shear for 30 minutes, then add DOP and furfural oil to shear for 15 minutes, stop shearing and keep at 170°C for 2 hours to obtain modified asphalt;

[0041] 2) preparing soap solution: heating water to 60-70° C., adding emulsifier and anhydrous calcium chloride in sequence and stirring evenly, and then adjusting the pH to 1-2 with hydrochloric acid to obtain soap solution;

[0042] 3) Preparation of high-solid content, high-viscosity and high-elastic modified emulsified asphalt: Start the high-speed shear instrument and stir the soap solution at a speed of 1500 r / min for 30 seconds, then increase to 7500 r / min, add the mixture of modified asphalt and warm mix agent to the soap solution and shear for 3 minutes. After shearing, quickly transfer to a colloid mill preheated at 60°C and grind for 30 seconds at a grinding speed of 3600 r / min to obtain high-solid content, high-viscosity and high-elastic modified emulsified asphalt.

[0043] Example 2

[0044] A high-solid content, high-viscosity and high-elastic modified emulsified asphalt comprises the following components in parts by mass: 100 parts of 90# road petroleum asphalt, 8 parts of star-shaped SBS (monomer ratio S / B is 4 / 6), 2.5 parts of rubber powder, 1.5 parts of DOP, 1 part of furfural oil, 2.5 parts of emulsifier, 3 parts of warm mix agent, 0.2 parts of anhydrous calcium chloride, 0.1 parts of hydrochloric acid and 55 parts of deionized water; the designed solid content is 62%.

[0045] The preparation method of the high-solid content, high-viscosity and high-elastic modified emulsified asphalt comprises the following steps:

[0046] 1) Preparation of modified asphalt: After heating 90# road petroleum asphalt to 150°C, add star-shaped SBS and rubber powder to swell for 15 minutes, start the high-speed shearing instrument and stir at a speed of 2500r / min and heat up. When the temperature rises to 185°C, increase the speed to 8000r / min and shear for 40 minutes, then add DOP and sulfur to shear for 20 minutes, stop shearing and keep at 185°C for 2.5 hours to obtain modified asphalt;

[0047] 2) preparing soap solution: heating water to 60-70° C., adding emulsifier and anhydrous calcium chloride in sequence and stirring evenly, and then adjusting the pH to 1-2 with hydrochloric acid to obtain soap solution;

[0048] 3) Preparation of high-solid content, high-viscosity and high-elastic modified emulsified asphalt: Start the high-speed shear instrument and stir the soap solution at a speed of 1500 r / min for 35 seconds, then increase to 7500 r / min, add the mixture of modified asphalt and warm mix agent to the soap solution and shear for 3 minutes. After shearing, quickly transfer to a colloid mill preheated at 70°C and grind for 40 seconds at a grinding speed of 4200 r / min to obtain high-solid content, high-viscosity and high-elastic modified emulsified asphalt.

[0049] Example 3

[0050] A high-solid content, high-viscosity and high-elastic modified emulsified asphalt comprises the following components in parts by weight: 100 parts of 70# road petroleum asphalt, 10 parts of linear SBS (monomer ratio S / B is 4 / 6), 2 parts of rubber powder, 0.6 parts of DOP, 1.5 parts of furfural oil, 2.5 parts of emulsifier, 2.5 parts of warm mix agent, 0.3 parts of anhydrous calcium chloride, 0.15 parts of hydrochloric acid, and 50 parts of deionized water; the designed solid content is 63%.

[0051] The preparation method of the high-solid content, high-viscosity and high-elastic modified emulsified asphalt comprises the following steps:

[0052] 1) Preparation of modified asphalt: After heating 70# road petroleum asphalt to 160°C, add linear SBS and rubber powder to swell for 10 minutes, start the high-speed shearing instrument and stir at 2500r / min and heat up. When the temperature rises to 175°C, increase the speed to 7000r / min and shear for 30 minutes, then add DOP and sulfur to shear for 15 minutes, stop shearing and keep at 170°C for 2 hours to obtain modified asphalt;

[0053] 2) preparing soap solution: heating water to 60-70° C., adding emulsifier and anhydrous calcium chloride in sequence and stirring evenly, and then adjusting the pH to 1-2 with hydrochloric acid to obtain soap solution;

[0054] 3) Preparation of high-solid content, high-viscosity and high-elastic modified emulsified asphalt: Start the high-speed shear instrument and stir the soap solution at a speed of 1000 r / min for 30 seconds, then increase to 8500 r / min, add the mixture of modified asphalt and warm mix agent to the soap solution and shear for 4 minutes. After shearing, quickly transfer to a colloid mill preheated at 70°C and grind for 50 seconds at a grinding speed of 6000 r / min to obtain high-solid content, high-viscosity and high-elastic modified emulsified asphalt.

[0055] Example 4

[0056] A high-solid content, high-viscosity and high-elastic modified emulsified asphalt comprises the following components in parts by mass: 100 parts of 70# road petroleum asphalt, 6 parts of emulsion SBR latex (solid content is 80%), 2.5 parts of rubber powder, 1 part of DOP, 0.5 parts of furfural oil, 2 parts of emulsifier, 4 parts of warm mix agent, 0.1 parts of anhydrous calcium chloride, 0.1 parts of hydrochloric acid and 50 parts of deionized water; the designed solid content is 68%.

[0057] The preparation method of the high-solid content, high-viscosity and high-elastic modified emulsified asphalt comprises the following steps:

[0058] 1) Preparation of modified asphalt: After heating 70# road petroleum asphalt to 140°C, SBR latex and rubber powder were added to swell for 15 minutes, and the high-speed shearing instrument was started to stir and heat at a speed of 2500r / min. When the temperature rose to 175°C, the speed was increased to 7000r / min for shearing for 30 minutes, and then DOP and sulfur were added for shearing for 15 minutes. After stopping the shearing, the modified asphalt was kept at 170°C for swelling for 2 hours to obtain the modified asphalt;

[0059] 2) preparing soap solution: heating water to 60-70° C., adding emulsifier and anhydrous calcium chloride in sequence and stirring evenly, and then adjusting the pH to 1-2 with hydrochloric acid to obtain soap solution;

[0060] 3) Preparation of high-solid content, high-viscosity and high-elastic modified emulsified asphalt: Start the high-speed shear instrument and stir the soap solution at a speed of 1500r / min for 40s, then increase to 7500r / min, add the mixture of modified asphalt and warm mix agent to the soap solution and shear for 4min, and quickly transfer to a colloid mill preheated at 70℃ and grind for 30s at a grinding speed of 4500r / min to obtain high-solid content, high-viscosity and high-elastic modified emulsified asphalt.

[0061] Example 5

[0062] A high-solid content, high-viscosity and high-elastic modified emulsified asphalt comprises the following components in parts by mass: 100 parts of 70# road petroleum asphalt, 8 parts of emulsion SBR latex (solid content is 80%), 3 parts of rubber powder, 1 part of DOP, 1.5 parts of furfural oil, 2 parts of emulsifier, 4 parts of warm mix agent, 0.2 parts of anhydrous calcium chloride, 0.1 parts of hydrochloric acid and 60 parts of deionized water; the designed solid content is 60%.

[0063] The preparation method of the high-solid content, high-viscosity and high-elastic modified emulsified asphalt comprises the following steps:

[0064] 1) Preparation of modified asphalt: After heating 70# road petroleum asphalt to 140°C, SBR latex and rubber powder were added to swell for 10 minutes, and the high-speed shearing instrument was started to stir and heat at a speed of 2500r / min. When the temperature rose to 175°C, the speed was increased to 7000r / min for shearing for 30 minutes, and then DOP and sulfur were added for shearing for 15 minutes. After stopping the shearing, the asphalt was kept at 170°C for swelling for 2 hours to obtain the modified asphalt;

[0065] 2) preparing soap solution: heating water to 60-70° C., adding emulsifier and anhydrous calcium chloride in sequence and stirring evenly, and then adjusting the pH to 1-2 with hydrochloric acid to obtain soap solution;

[0066] 3) Preparation of high-solid content, high-viscosity and high-elastic modified emulsified asphalt: Start the high-speed shear instrument and stir the soap solution at a speed of 2000 r / min for 55 seconds, then increase to 8000 r / min, add the mixture of modified asphalt and warm mix agent to the soap solution and shear for 3.5 minutes. After shearing, quickly transfer to a colloid mill preheated at 70°C and grind for 40 seconds at a grinding speed of 6000 r / min to obtain high-solid content, high-viscosity and high-elastic modified emulsified asphalt.

[0067] The actual solid content and storage stability of the high-solid content, high-viscosity and high-elastic modified emulsified asphalt in Examples 1-5 were tested, and interlayer shear test and direct pull test were designed to test its adhesion and toughness.

[0068] The specific method of the interlayer shear test is as follows: take a rutting plate of AC-13 asphalt mixture with a length of 300mm×width of 300mm×thickness of 25mm, and after curing at room temperature for three days, spray the modified emulsified asphalt with high solid content, high viscosity and high elasticity on the rutting plate with a thickness of 25mm. After curing for one day to break the emulsion, add 25mm thick AC-20 asphalt mixture to make a standard rutting plate with a length of 300mm×width of 300mm×thickness of 50mm, and then use a coring machine to take out a cylindrical specimen with a diameter of 100mm and a height of 50mm; the cylindrical specimen is tested for interlayer strength using a universal testing machine UTM-100.

[0069] The specific method of the direct pull-out test is as follows: apply high-solid content, high-viscosity and high-elastic modified emulsified asphalt on limestone with a length of 50mm×width of 50mm×thickness of 10mm, and control the thickness of the asphalt film to 0.2mm. Align and bond two pieces of limestone coated with emulsified asphalt together, and make a pull-out specimen after curing for three days; use the universal testing machine UTM-100 to test the direct pull-out force value and asphalt elongation of the pull-out specimen.

[0070] Table 1

[0071]

[0072] It can be seen from the test results in Table 1 that the modified emulsified asphalt prepared by the present invention has a higher solid content, as well as higher viscosity and elasticity, and has excellent comprehensive performance.

[0073] The above embodiments are merely examples for clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above descriptions. It is not necessary and impossible to list all the implementation methods here, and the obvious changes or modifications derived therefrom are still within the protection scope of the invention.

Claims

1. A method for preparing a high-solid content, high-viscosity and high-elastic modified emulsified asphalt. It is characterized in that The following steps are involved: 1) Preparation of modified asphalt: After heating the base asphalt to 140-160°C, add the modifier and elasticizer to swell for 10-20 minutes, start the high-speed shearing instrument and stir and heat at a speed of 2000-3000 r / min, when the temperature rises to 175-200°C, increase the speed to 7000-9000 r / min and shear for 30-60 minutes, then add the plasticizer and stabilizer to shear for 15-30 minutes, stop shearing, keep warm at 170-190°C for 2-3 hours to obtain modified asphalt; 2) preparing soap solution: heating water, adding emulsifier and co-emulsifier in sequence and stirring evenly, and then adjusting the pH with a pH adjuster to obtain soap solution; 3) Preparation of high-solid content, high-viscosity and high-elastic modified emulsified asphalt: Start the high-speed shear instrument and stir the soap solution at a speed of 1000-2000 r / min for 30-60s, then increase to 7000-8500 r / min, add the mixture of modified asphalt and warm mix agent into the soap solution and shear for 3-4 minutes, and after shearing, quickly transfer to a colloid mill preheated at 50-70°C and grind at 2000-6500 r / min for 30-40s to obtain high-solid content, high-viscosity and high-elastic modified emulsified asphalt; The high-solid content, high-viscosity and high-elasticity modified emulsified asphalt comprises the following components in parts by mass: 100 parts of base asphalt, 8-10 parts of modifier, 2-4 parts of elasticizer, 0.5-1.5 parts of plasticizer, 0.5-1.5 parts of stabilizer, 1.5-5 parts of emulsifier, 2-8 parts of warm mix agent, 0.1-0.3 parts of auxiliary emulsifier, 0.1-0.2 parts of pH regulator, and 40-70 parts of water; the modifier is SBS or SBR; the elasticizer is rubber powder; the plasticizer is dioctyl phthalate or dibutyl phthalate; the warm mix agent is Sasobite; the stabilizer is furfural oil; the solid content of the high-solid content, high-viscosity and high-elasticity modified emulsified asphalt is 60-75%.

2. The method for preparing the high-solid content, high-viscosity and high-elastic modified emulsified asphalt according to claim 1, It is characterized in that The SBS is star-shaped or linear; the SBR is emulsion SBR latex or emulsion SBR powder; the solid content of the emulsion SBR latex is 60-90%.

3. The method for preparing the high-solid content, high-viscosity and high-elastic modified emulsified asphalt according to claim 1, It is characterized in that The matrix asphalt is one of 50#, 70# and 90# road petroleum asphalt.

4. The method for preparing the high-solid content, high-viscosity and high-elastic modified emulsified asphalt according to claim 1, It is characterized in that The emulsifier is a slow-cracking, fast-setting cationic asphalt emulsifier; the auxiliary emulsifier is anhydrous calcium chloride, and the pH regulator is hydrochloric acid.

5. The method for preparing the high-solid content, high-viscosity and high-elastic modified emulsified asphalt according to claim 1, It is characterized in that The heating temperature of the water is 60-70° C., and the pH of the soap solution is 1-2.

Citation Information

Patent Citations

  • Styrene-butadiene rubber modified asphalt mixture and preparation method thereof

    CN104371340A

  • Preparation method of high-solid-content emulsified SBS (styrene-butadiene-styrene) modified asphalt and application of modified asphalt in micro-surfacing

    CN104387594A

  • Emulsified asphalt material with high solid content and preparation method of emulsified asphalt material

    CN106832974A

  • SBS high-viscosity modified emulsified asphalt material and preparation process thereof

    CN111286209A

  • Micro-surfacing emulsified asphalt suitable for low-temperature construction at night as well as preparation method and application thereof

    CN111849179A