Silicon-containing vegetable oil-based dual UV curing material and preparation method and application thereof
By chemically modifying ricinoleic acid and epoxidized vegetable oil and adding a composite photoinitiator, a silicon-containing vegetable oil-based dual UV curable material was prepared, which solved the problems of slow curing speed and high resource consumption in the existing technology, and achieved High-efficiency, low resource consumption photo-curing effect, suitable for UV curing coatings, inks and adhesives.
Patent Information
- Application Number
- CN202310527549.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-05-10
AI Technical Summary
Existing UV curable materials have slow curing speed, large shrinkage rate, and obvious oxygen inhibition effect, making it difficult to meet the needs of rapid curing and low resource consumption.
A silicon-containing vegetable oil-based dual UV curing material is prepared by chemically modifying ricinoleic acid and epoxidized vegetable oil, and adding a composite photoinitiator and reactive diluent to form a material with low viscosity, high adhesion, acid resistance and resistance to Photo-curable film with good boiling water resistance utilizes the synergistic effect of free radicals and cationic photoinitiators to achieve rapid curing.
It achieves high cross-linking degree, transparency and good mechanical properties of the photo-cured film, reduces the use of petrochemical resources, and improves the performance and application scope of vegetable oil in photo-cured coatings.
Smart Images

Figure CN116640261B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of UV curing materials, and in particular to a silicon-containing vegetable oil-based dual UV curing material and a preparation method and application thereof. Background Art
[0002] The depletion of fossil resources and environmental pollution are gradually becoming more serious. As a renewable resource and biodegradable material, vegetable oil materials are attracting people's attention. my country's soybean oil, castor oil and tung oil are abundant and cheap, and have excellent improvement potential because of their multiple functional groups. Converting vegetable oil into more valuable materials can not only reduce dependence on fossil resources, but also increase the added value of vegetable oil. Based on the requirements of energy saving, environmental protection, sustainability and high performance, it is of great practical significance to develop new UV curing materials with fast curing and excellent performance.
[0003] UV curing refers to the use of medium and short waves (300-800nm) of UV light. Under UV radiation, the photoinitiator absorbs the radiation energy of ultraviolet light and splits into free radicals, which triggers the polymerization, cross-linking and grafting reactions of prepolymers, and solidifies into a network polymer in a very short time. As a result, UV coatings, inks, adhesives, etc. are converted from liquid to solid within a few seconds to form a pattern. It is a new technology that emerged in the 1960s, is environmentally friendly, and has low VOC emissions.
[0004] The two commonly used UV curing methods are free radical curing and cationic curing. Cationic active species have a long life and are still active after the exposure is terminated. They can continue to induce cross-linking and curing of photosensitive resins, but the disadvantage is that the curing speed is slow. Among them, free radical photocuring has the advantage of fast reaction speed, but the disadvantages are large curing shrinkage and oxygen inhibition effect. Summary of the invention
[0005] In view of the problems raised by the background technology, the purpose of the present invention is to propose a method for preparing a silicon-containing vegetable oil-based dual UV curing material. The prepared silicon-containing vegetable oil-based dual UV curing material has the characteristics of low viscosity, high adhesion, good acid resistance and boiling water resistance, high transparency and fast curing speed. The photocured film formed after photocuring has a high degree of crosslinking, transparency and good mechanical properties. The ricinoleic acid and epoxy vegetable oil, which are rich bio-based raw materials, are introduced into the photocuring coating, reducing the use of petrochemical resources in the photocuring coating.
[0006] Another object of the present invention is to provide a silicon-containing vegetable oil-based dual UV curing material prepared using the above preparation method, which has the characteristics of low viscosity, high adhesion, good acid resistance and boiling water resistance, high transparency and fast curing speed.
[0007] Another object of the present invention is to propose the application of the above-mentioned silicon-containing vegetable oil-based dual UV curing material in UV curing coatings, UV curing inks and UV curing adhesives, which has a wide range of applications and strong applicability.
[0008] To achieve this object, the present invention adopts the following technical solutions:
[0009] A method for preparing a silicon-containing vegetable oil-based dual UV curing material comprises the following steps:
[0010] Step (1), preparation of castor oil-based polysiloxane: stir ricinoleic acid, acid anhydride and catalyst at 75-95° C. in a nitrogen atmosphere for 2-4 hours, add silane coupling agent KH-560 and inhibitor to continue reaction, and obtain castor oil-based polysiloxane;
[0011] Step (2), preparation of epoxidized vegetable oil-based acrylate: stirring hydroxyethyl acrylate, acid anhydride and catalyst at 75-95° C. for 2-4 hours, adding epoxidized vegetable oil and inhibitor to continue the reaction, and obtaining epoxidized vegetable oil-based acrylate;
[0012] Step (3), mixing castor oil-based polysiloxane with epoxidized vegetable oil-based acrylate, adding a composite photoinitiator and a reactive diluent and mixing evenly to obtain a silicon-containing vegetable oil-based dual UV curing material;
[0013] The composite photoinitiator includes a free radical photoinitiator and a cationic photoinitiator.
[0014] To further illustrate, in the step (3), 10 to 60% of castor oil-based polysiloxane and 10 to 60% of epoxidized vegetable oil-based acrylate are mixed according to the mass percentage, and 1 to 10% of a composite photoinitiator and 10 to 50% of a reactive diluent are added and mixed evenly to obtain a silicon-containing vegetable oil-based dual UV curing material.
[0015] To further illustrate, in step (3), the mass ratio of castor oil-based polysiloxane to epoxidized vegetable oil-based acrylate is (1-4): (1-4).
[0016] Further, in the step (1), ricinoleic acid, anhydride and catalyst are stirred at 75-95° C. in a nitrogen atmosphere for 2-4 hours, silane coupling agent KH-560 and polymerization inhibitor are added, and the catalyst is added and then the reaction is continued, and the mixture is stirred at 70-90° C. for 5-12 hours to obtain castor oil-based polysiloxane;
[0017] In the step (1), the molar ratio of the ricinoleic acid, the acid anhydride and the silane coupling agent KH-560 is 1:(1-2.5):(1-2.5), the added amount of the catalyst is 0.4-2% of the total mass of the ricinoleic acid, the acid anhydride and the silane coupling agent KH-560, and the added amount of the inhibitor is 0.01-1% of the total mass of the ricinoleic acid, the acid anhydride and the silane coupling agent KH-560.
[0018] Further, in the step (2), hydroxyethyl acrylate, anhydride and catalyst are stirred at 75-95° C. for 2-4 hours, epoxidized vegetable oil and inhibitor are added, and the catalyst is added and then the reaction is continued, and the reaction is stirred at 75-95° C. for 4-6 hours to obtain epoxidized vegetable oil-based acrylate;
[0019] In the step (2), the molar ratio of the epoxidized vegetable oil, the acid anhydride and the hydroxyethyl acrylate is 1:(1-2.5):(1-2.5), the added amount of the catalyst is 0.5-2.5% of the total mass of the epoxidized vegetable oil, the acid anhydride and the hydroxyethyl acrylate, and the added amount of the inhibitor is 0.01-0.08% of the total mass of the epoxidized vegetable oil, the acid anhydride and the hydroxyethyl acrylate.
[0020] Further, in step (2), the epoxidized vegetable oil is any one or more of epoxidized rapeseed oil, epoxidized castor oil, epoxidized palm oil and epoxidized soybean oil;
[0021] In the step (1) and the step (2), the acid anhydride is any one or more of a combination of maleic anhydride, succinic anhydride and phthalic anhydride, the catalyst is any one or more of a combination of N,N-dimethylbenzylamine, triethylamine, tetrabutylammonium bromide and triphenylphosphine, and the inhibitor is any one or more of a combination of hydroquinone, 4-methoxyphenol, 2,5-di-tert-butyl-p-cresol and tert-butylhydroquinone.
[0022] Further, in the step (3), the composite photoinitiator is composed of a free radical photoinitiator and a cationic photoinitiator, and the mass ratio of the free radical photoinitiator to the cationic photoinitiator is (1-9): (1-9);
[0023] The free radical photoinitiator is any one or more combinations of 2-hydroxy-2-methyl-phenylacetone-1, 1-hydroxy-cyclohexyl benzophenone, 2-hydroxy-2-methyl-p-hydroxyethyl ether phenylacetone-1, 2-methyl-1-(4-methylthiophenyl)-2-morpholinyl-1-propanone, 2,4,6-trimethylbenzoyl-ethoxy-phenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide and 4-p-toluenethiodibenzophenone, and the cationic photoinitiator is any one or more combinations of diazonium salts, diaryliodonium salts, triarylsulfonium salts, alkylsulfonium salts, iron arene salts, sulfonyloxy ketones and triarylsiloxane ethers.
[0024] To further illustrate, in step (3), the reactive diluent is a combination of any one or more of tripropylene glycol diacrylate, 1,6-hexanediol diacrylate, glycidyl acrylate and glycidyl methacrylate.
[0025] A silicon-containing vegetable oil-based dual UV curing material is prepared by the method for preparing the silicon-containing vegetable oil-based dual UV curing material.
[0026] The silicon-containing vegetable oil-based dual UV curing material is used in UV curing coatings, UV curing inks and UV curing adhesives.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] The preparation method of the silicon-containing vegetable oil-based dual UV curing material is characterized by low viscosity, high adhesion, good acid resistance and boiling water resistance, high transparency, and fast curing speed. The photocured film formed after photocuring has high crosslinking degree, transparency, and good mechanical properties. The vegetable oil is effectively used in photocuring coatings, which reduces the use of petroleum-based raw materials and reduces the use of petrochemical resources. Increasing functionality through chemical modification can increase the crosslinking density of silicon-containing vegetable oil-based photocuring coatings, thereby improving the performance of vegetable oil-based photocuring films; on the other hand, the use of vegetable oil in photocuring coatings can effectively reduce the use of petrochemical resources in photocuring coatings. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a synthetic route of the castor oil-based polysiloxane of Example 1 of the present invention (in the figure, RA is ricinoleic acid, MA is maleic anhydride, TBAB is tetrabutylammonium bromide, PPh3 is triphenylphosphine, MAR is ricinoleic acid acrylate, GPTMA is silane coupling agent KH-560, and MARGP is castor oil-based polysiloxane).
[0030] Figure 2This is a synthetic route of the epoxidized vegetable oil-based acrylate of Example 1 of the present invention (in the figure, HEA is hydroxyethyl acrylate, MA is maleic anhydride, TBAB is tetrabutylammonium bromide, MAH is hydroxyethyl acrylate maleic acid half ester, ESO is epoxidized soybean oil, PPh3 is triphenylphosphine, and MAHE is epoxidized soybean oil acrylate).
[0031] Figure 3 : is the infrared spectrum of castor oil-based polysiloxane MARGP of Example 1 of the present invention, in which R1, R2, R3, and R4 represent the cured films of Example 1, Example 2, Example 3, and Example 4 after curing, respectively).
[0032] Figure 4 This is the infrared spectrum of the epoxy soybean oil acrylate MAHE in Example 1 of the present invention.
[0033] Figure 5 3. Strain-stress diagram of photocured films made from photocured materials obtained in Examples 1-4 of the present invention (in the figure, R1, R2, R3, and R4 represent Example 1, Example 2, Example 3, and Example 4, respectively).
[0034] Figure 6 1 is a shear rate-viscosity diagram of the photocurable films made from the photocurable materials obtained in Examples 1-4 of the present invention (in the diagram, R1, R2, R3, and R4 represent Example 1, Example 2, Example 3, and Example 4, respectively).
[0035] Figure 7 This is a graph showing how the glass transition temperature of the photocurable materials of Examples 1-5 of the present invention changes with temperature (in the graph, R1, R2, R3, R4, and R5 represent Example 1, Example 2, Example 3, Example 4, and Example 5, respectively).
[0036] Figure 8 Graph showing the variation of storage modulus (E') of the photocurable materials of Examples 1-5 of the present invention with temperature (in the graph, R1, R2, R3, R4, and R5 represent Example 1, Example 2, Example 3, Example 4, and Example 5, respectively).
[0037] Fig. 9 These are observation pictures of digital macroscopic morphology after coating with the photocurable materials of Examples 1, 3 and 4 of the present invention (in the picture, R1, R3, R4 represent Example 1, Example 3, Example 4 respectively, and R0 is a picture of the covered glass plate). DETAILED DESCRIPTION
[0038] A method for preparing a silicon-containing vegetable oil-based dual UV curing material comprises the following steps:
[0039] Step (1), preparation of castor oil-based polysiloxane: stir ricinoleic acid, acid anhydride and catalyst at 75-95° C. in a nitrogen atmosphere for 2-4 hours, add silane coupling agent KH-560 and inhibitor to continue reaction, and obtain castor oil-based polysiloxane;
[0040] Step (2), preparation of epoxidized vegetable oil-based acrylate: stirring hydroxyethyl acrylate, acid anhydride and catalyst at 75-95° C. for 2-4 hours, adding epoxidized vegetable oil and inhibitor to continue the reaction, and obtaining epoxidized vegetable oil-based acrylate;
[0041] Step (3), mixing castor oil-based polysiloxane with epoxidized vegetable oil-based acrylate, adding a composite photoinitiator and a reactive diluent and mixing evenly to obtain a silicon-containing vegetable oil-based dual UV curing material;
[0042] The composite photoinitiator includes a free radical photoinitiator and a cationic photoinitiator.
[0043] The invention adopts unsaturated vegetable oil ricinoleic acid and acid anhydride to carry out an anhydride reaction to prepare ricinoleic acid-based dibasic acid with a long fatty acid chain, and carries out a ring-opening reaction between the ricinoleic acid-based dibasic acid and a silane coupling agent KH-560 having an epoxy group to prepare a multifunctional unsaturated castor oil-based polysiloxane containing silicon. At the same time, hydroxyethyl acrylate and acid anhydride are used to carry out an anhydride reaction, and then a ring-opening reaction is carried out with an epoxidized vegetable oil containing multiple epoxy groups to prepare a silicon-containing vegetable oil-based dual UV curing material. The castor oil-based polysiloxane and the epoxidized vegetable oil-based acrylate are uniformly mixed to obtain a multifunctional vegetable oil-based prepolymer, i.e., a silicon-containing vegetable oil-based dual UV curing material prepolymer, and a composite photoinitiator and a reactive diluent are added to obtain the silicon-containing vegetable oil-based dual UV curing material. On the one hand, the multifunctional unsaturated castor oil-based polysiloxane has active double bonds that can undergo free radical polymerization. At the same time, silane coupling agent KH-560 is added to castor oil acrylate to introduce silicon. Silicon and carbon both belong to the IVA main group and are easy to form SP 3 The hybrid orbital is tetrahedral in shape. The silicon atom has a larger radius and an empty 3d orbital. Compared with the carbon atom, its electronegativity is smaller, and the Si-Y covalent bond formed is ionic. Therefore, it can also react with OH under mild conditions. -1, double bonds and other substances. Two of the four covalent bonds formed with silicon atoms are combined with oxygen atoms, forming a linear molecular structure of repeating units. The remaining two covalent bonds are connected to various organic groups. Therefore, polysiloxane has the characteristics of heat resistance, weather resistance, water resistance, low surface energy and surface tension. The traditional curing method of silicone materials has a long curing speed and low efficiency, which is not conducive to large-scale production. By introducing silicone into the photosensitive group and then using UV light curing, it is possible to achieve fast and energy-saving curing while maintaining excellent performance. In addition, the silicon-containing vegetable oil-based dual UV curing material of the present invention contains a large amount of silicon element, the color transparency of the cured material is high, and the cross-linking density network is dense, which increases the glass transition temperature. Due to the simultaneous addition of free radical photoinitiator and cationic photoinitiator, the purpose of free radical / cationic dual curing is achieved. The hybrid curing technology can synthesize UV-curable adhesives with excellent performance, so that different types of polymerization reactions occur between molecules of the same type. The products after polymerization contain more cross-linking modes, which are transmitted to each other through linear and network structures, making the molecular weight of the produced polymer more uniform, and the performance of the cured product is greatly improved.
[0044] On the other hand, the addition of epoxidized vegetable oil is beneficial to improving the functionality of silicon-containing vegetable oil-based dual-curing materials and increasing the cross-linking density of the polymer, thereby improving the relevant properties of the cured film. By adjusting the ratio of epoxidized vegetable oil-based acrylate to castor oil-based polysiloxane, materials with different mechanical properties can be obtained.
[0045] The silicon-containing vegetable oil-based dual UV curing material prepared by the preparation method of the silicon-containing vegetable oil-based dual UV curing material of the present invention has a photopolymerization cross-linking polymerization reaction of three groups, carbon-carbon double bond, epoxy group, and silicon oxygen bond, during the curing process. The three photocuring groups have a synergistic copolymerization effect, wherein the carbon-carbon double bond generates free radicals and cations, the epoxy group generates a cationic photocuring reaction, and the silicon oxygen bond generates a sol-gel reaction. After curing, the polymer networks are entangled with each other to form an interpenetrating polymer network. The specific curing reaction mechanism formed by the three is as follows: during the ultraviolet curing process, the free radical type photoinitiator is excited by ultraviolet radiation to become a free radical active body, and the active body reacts with the carbon-carbon double bond of castor oil-based polysiloxane and epoxidized vegetable oil-based acrylate. At the same time, there is a self-polymerization reaction of the two prepolymers themselves to form a growth chain. As the illumination time increases, the growth chain further reacts to form a longer polymer chain. At the same time, the epoxy group in the epoxidized vegetable oil-based acrylate undergoes ring-opening polymerization. Since cationic polymerization and free radical polymerization occur on the same molecule, a polymerized whole with strong chemical bonds is formed after curing, so that the volume complementary effect of free radicals and cations is transmitted through chemical bonds, thereby improving the performance of UV-cured adhesives. Cationic curing and free radical curing have synergistic polymerization effects. At the same time, the Si-O bonds in castor oil-based polysiloxane are converted into Si-O-Si bonds through hydrolysis / condensation, and the side chains contain more active hydrogen atoms, thereby improving the flexibility and elongation at break of the photocured film. The three polymerization methods form a cross-linked network that entangles with each other, causing the molecular weight of the system to increase continuously, and finally forming a cured film.
[0046] Furthermore, the present invention utilizes abundant bio-based raw materials such as ricinoleic acid and epoxidized vegetable oil to introduce into acrylate, which can effectively reduce the utilization of petrochemical resources. By selecting epoxidized vegetable oil, ricinoleic acid, acid anhydride and other biomass-rich, cheap, and biodegradable materials to replace petrochemical resources, the crisis of tight petrochemical resources can be alleviated, and the application field of biomass in photocuring coatings can be broadened, which has a positive reference role.
[0047] The invention discloses a method for preparing a silicon-containing vegetable oil-based dual UV curing material. The prepared silicon-containing vegetable oil-based dual UV curing material has the characteristics of low viscosity, high adhesion, good acid resistance and boiling water resistance, high transparency and fast curing speed. The photocured film formed after photocuring has high crosslinking degree, transparency and good mechanical properties. The vegetable oil is effectively introduced into the photocuring coating, and the use of petroleum-based raw materials is reduced.
[0048] To further illustrate, in the step (3), 10 to 60% of castor oil-based polysiloxane and 10 to 60% of epoxidized vegetable oil-based acrylate are mixed according to the mass percentage, and 1 to 10% of a composite photoinitiator and 10 to 50% of a reactive diluent are added and mixed evenly to obtain a silicon-containing vegetable oil-based dual UV curing material.
[0049] Preferably, in step (3), the mass ratio of castor oil-based polysiloxane to epoxidized vegetable oil-based acrylate is (1-4): (1-4).
[0050] By adjusting the ratio of epoxidized vegetable oil-based acrylate to castor oil-based polysiloxane, materials with different mechanical properties can be obtained. By continuously increasing the content of castor oil-based polysiloxane, the pencil hardness of the cured photocured film will gradually increase and the tensile strength will increase.
[0051] Further, in the step (1), ricinoleic acid, anhydride and catalyst are stirred at 75-95° C. in a nitrogen atmosphere for 2-4 hours, silane coupling agent KH-560 and polymerization inhibitor are added, and the catalyst is added and then the reaction is continued, and the mixture is stirred at 70-90° C. for 5-12 hours to obtain castor oil-based polysiloxane;
[0052] In the step (1), the molar ratio of the ricinoleic acid, the acid anhydride and the silane coupling agent KH-560 is 1:(1-2.5):(1-2.5), the added amount of the catalyst is 0.4-2% of the total mass of the ricinoleic acid, the acid anhydride and the silane coupling agent KH-560, and the added amount of the inhibitor is 0.01-1% of the total mass of the ricinoleic acid, the acid anhydride and the silane coupling agent KH-560.
[0053] Further, in the step (2), hydroxyethyl acrylate, anhydride and catalyst are stirred at 75-95° C. for 2-4 hours, epoxidized vegetable oil and inhibitor are added, and the catalyst is added and then the reaction is continued, and the reaction is stirred at 75-95° C. for 4-6 hours to obtain epoxidized vegetable oil-based acrylate;
[0054] In the step (2), the molar ratio of the epoxidized vegetable oil, the acid anhydride and the hydroxyethyl acrylate is 1:(1-2.5):(1-2.5), the added amount of the catalyst is 0.5-2.5% of the total mass of the epoxidized vegetable oil, the acid anhydride and the hydroxyethyl acrylate, and the added amount of the inhibitor is 0.01-0.08% of the total mass of the epoxidized vegetable oil, the acid anhydride and the hydroxyethyl acrylate.
[0055] Specifically, in step (2), the epoxidized vegetable oil is any one or more of epoxidized rapeseed oil, epoxidized castor oil, epoxidized palm oil and epoxidized soybean oil;
[0056] In the step (1) and the step (2), the acid anhydride is any one or more of a combination of maleic anhydride, succinic anhydride and phthalic anhydride, the catalyst is any one or more of a combination of N,N-dimethylbenzylamine, triethylamine, tetrabutylammonium bromide and triphenylphosphine, and the inhibitor is any one or more of a combination of hydroquinone, 4-methoxyphenol, 2,5-di-tert-butyl-p-cresol and tert-butylhydroquinone.
[0057] Preferably, in step (3), the composite photoinitiator is composed of a free radical photoinitiator and a cationic photoinitiator, and the mass ratio of the free radical photoinitiator to the cationic photoinitiator is (1-9): (1-9);
[0058] The free radical photoinitiator is any one or more combinations of 2-hydroxy-2-methyl-phenylacetone-1, 1-hydroxy-cyclohexyl benzophenone, 2-hydroxy-2-methyl-p-hydroxyethyl ether phenylacetone-1, 2-methyl-1-(4-methylthiophenyl)-2-morpholinyl-1-propanone, 2,4,6-trimethylbenzoyl-ethoxy-phenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide and 4-p-toluenethiodibenzophenone, and the cationic photoinitiator is any one or more combinations of diazonium salts, diaryliodonium salts, triarylsulfonium salts, alkylsulfonium salts, iron arene salts, sulfonyloxy ketones and triarylsiloxane ethers.
[0059] The present invention can synthesize ultraviolet light-cured adhesive with excellent performance by using free radical / cationic dual curing technology, so that different types of polymerization reactions occur between molecules of the same type, and the cross-linking modes contained in the product after polymerization are increased, and the molecular weight of the generated polymer is more uniform through the transmission of linear and mesh structures, and the performance of the product after curing is greatly improved. In addition, by using the synthesis of organic-inorganic sol-gel materials, triarylsulfonium salts are used as cationic photoinitiators to achieve organic-inorganic UV curing of epoxy and trimethoxysilane, and sol-gel polycondensation is achieved at the same time. Using triarylsulfonium salts as superacid photoinitiators, epoxy ring opening of epoxidized vegetable oil-based acrylates and sol-gel polymerization of castor oil-based polysiloxane can be initiated simultaneously, and the double bond polymerization of the free radical photoinitiator is coordinated at the same time, thereby effectively promoting the increase of light curing speed, thereby improving curing efficiency.
[0060] Specifically, in the step (3), the reactive diluent is any one or more of tripropylene glycol diacrylate, 1,6-hexanediol diacrylate, glycidyl acrylate and glycidyl methacrylate.
[0061] A silicon-containing vegetable oil-based dual UV curing material is prepared by the method for preparing the silicon-containing vegetable oil-based dual UV curing material.
[0062] The silicon-containing vegetable oil-based dual UV curing material is used in UV curing coatings, UV curing inks and UV curing adhesives.
[0063] The method for using the silicon-containing vegetable oil-based dual UV curing material is as follows: after coating the silicon-containing vegetable oil-based dual UV curing material, irradiate it under ultraviolet light for photocuring reaction, the wavelength of the ultraviolet light is 245nm to 430nm (preferably the wavelength of the ultraviolet light is 365nm), and the irradiation time is 1 to 5 minutes. The silicon-containing vegetable oil-based dual UV curing material can be used as a coating in the fields of coatings, inks, adhesives, plastics, fibers and composite materials, and has a wide range of applications and strong applicability.
[0064] In order to facilitate the understanding of the present invention, the present invention is described more fully below. The present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0065] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0066] Example 1
[0067] A method for preparing a silicon-containing vegetable oil-based dual UV curing material comprises the following steps:
[0068] Step (1), preparation of castor oil-based polysiloxane: 30 g of castor oil acid, 10 g of acid anhydride (maleic anhydride, purity 99%) and 0.4 g of catalyst (tetrabutylammonium bromide) were added to a three-necked flask with a thermometer, stirred at 90° C. in a nitrogen atmosphere for 3 h, 47 g of silane coupling agent KH-560 (purity 97%) and 0.02 g of polymerization inhibitor (4-methoxyphenol) were slowly added dropwise, 0.87 g of catalyst (triphenylphosphine) was added, and the reaction was continued at 75° C. for 10 h to obtain castor oil-based polysiloxane (MARGP);
[0069] The molar ratio of ricinoleic acid, acid anhydride and silane coupling agent KH-560 is 1:1:2, the amount of catalyst added is 1.5% of the total mass of ricinoleic acid, acid anhydride and silane coupling agent KH-560 (the amount of tetrabutylammonium bromide added is 1% of the total mass of ricinoleic acid and acid anhydride, and the amount of triphenylphosphine added is 1% of the total mass of ricinoleic acid, acid anhydride and silane coupling agent KH-560), and the amount of inhibitor added is 0.02% of the total mass of ricinoleic acid, acid anhydride and silane coupling agent KH-560;
[0070] Step (2), preparation of epoxidized vegetable oil-based acrylate: 12 g of hydroxyethyl acrylate, 10 g of acid anhydride (maleic anhydride, purity 99%) and 0.22 g of catalyst (tetrabutylammonium bromide) were added to a three-necked flask with a thermometer, stirred at 90° C. for 2.5 h, 27 g of epoxidized vegetable oil (epoxidized soybean oil, purity 97%) and 0.02 g of inhibitor (4-methoxyphenol) were slowly added dropwise, 0.49 g of catalyst (triphenylphosphine) was added, and the reaction was continued at 80° C. for 5 h to obtain epoxidized vegetable oil-based acrylate (epoxidized soybean oil acrylate, MAHE);
[0071] The molar ratio of the epoxidized vegetable oil, the acid anhydride and the hydroxyethyl acrylate is 1:1:1, the amount of the catalyst added is 1.4% of the total mass of the epoxidized vegetable oil, the acid anhydride and the hydroxyethyl acrylate (the amount of tetrabutylammonium bromide added is 1% of the total mass of the epoxidized vegetable oil and the acid anhydride, and the amount of triphenylphosphine added is 1% of the total mass of the epoxidized vegetable oil, the acid anhydride and the hydroxyethyl acrylate), and the amount of the inhibitor added is 0.04% of the total mass of the epoxidized vegetable oil, the acid anhydride and the hydroxyethyl acrylate;
[0072] Step (3), mixing 1 g of castor oil-based polysiloxane (MARGP) with 4 g of epoxidized vegetable oil-based acrylate (MAHE), adding 0.2 g of a composite photoinitiator and 4 g of a reactive diluent and mixing evenly to obtain a silicon-containing vegetable oil-based dual UV curing material;
[0073] Among them, calculated by mass percentage, the addition amount of castor oil-based polysiloxane is 10.8%, the addition amount of epoxidized vegetable oil-based acrylate is 43.5%, the addition amount of composite photoinitiator is 2.2%, and the addition amount of active diluent is 43.5%; the mass ratio of castor oil-based polysiloxane to epoxidized vegetable oil-based acrylate is 1:4;
[0074] The composite photoinitiator is composed of a free radical photoinitiator and a cationic photoinitiator, wherein the free radical photoinitiator uses 2-hydroxy-2-methyl-phenylacetone-1, and the addition amount is 1g; the cationic photoinitiator uses diphenyl-(4-phenylthio)phenylsulfonium hexafluorophosphate, and the addition amount is 1g; the mass ratio of the free radical photoinitiator to the cationic photoinitiator is 1:1;
[0075] As the reactive diluent, 2 g of tripropylene glycol diacrylate (TPGDA) and 2 g of 1,6-hexanediol diacrylate (HDDA) were used.
[0076] Example 2
[0077] A method for preparing a silicon-containing vegetable oil-based dual UV curing material. Compared with Example 1, in step (3) of Example 2, the added amount of castor oil-based polysiloxane is 2 g, the added amount of epoxidized vegetable oil-based acrylate is 3 g, the mass ratio of castor oil-based polysiloxane to epoxidized vegetable oil-based acrylate is 2:3, and the remaining preparation methods and raw materials are consistent with Example 1, thereby obtaining a silicon-containing vegetable oil-based dual UV curing material.
[0078] Example 3
[0079] A method for preparing a silicon-containing vegetable oil-based dual UV curing material. Compared with Example 1, in step (3) of Example 3, the added amount of castor oil-based polysiloxane is 3g, the added amount of epoxidized vegetable oil-based acrylate is 2g, the mass ratio of castor oil-based polysiloxane to epoxidized vegetable oil-based acrylate is 3:2, and the remaining preparation methods and raw materials are consistent with Example 1, thereby obtaining a silicon-containing vegetable oil-based dual UV curing material.
[0080] Example 4
[0081] A method for preparing a silicon-containing vegetable oil-based dual UV curing material. Compared with Example 1, in step (3) of Example 4, the added amount of castor oil-based polysiloxane is 4g, the added amount of epoxidized vegetable oil-based acrylate is 1g, the mass ratio of castor oil-based polysiloxane to epoxidized vegetable oil-based acrylate is 4:1, and the remaining preparation methods and raw materials are consistent with Example 1, thereby obtaining a silicon-containing vegetable oil-based dual UV curing material.
[0082] Example 5
[0083] A method for preparing a silicon-containing vegetable oil-based dual UV curing material. Compared with Example 1, in step (3) of Example 5, the added amount of castor oil-based polysiloxane is 2.5 g, the added amount of epoxidized vegetable oil-based acrylate is 2.5 g, the mass ratio of castor oil-based polysiloxane to epoxidized vegetable oil-based acrylate is 1:1, and the remaining preparation methods and raw materials are consistent with Example 1, thereby obtaining a silicon-containing vegetable oil-based dual UV curing material.
[0084] Performance test: The silicon-containing vegetable oil-based dual UV curing material prepared in Examples 1-5 was coated on a tinplate using a 500 μm thick applicator, and irradiated under ultraviolet light of 365 nm wavelength for 2 min to obtain a multifunctional epoxy soybean oil acrylate photocurable film, and the following tests were performed:
[0085] 1. Infrared spectrum detection: Infrared spectrum detection was performed on the intermediate product (castor oil-based polysiloxane) obtained in Example 1 and the cured films after photocuring in Examples 1 to 4 to perform infrared comparison before and after curing of the photocurable materials. Infrared spectrum detection was performed on the epoxidized vegetable oil-based acrylate (epoxidized soybean oil acrylate) obtained in Example 1. The results are as follows:
[0086] like Figure 3 As shown, 1168cm -1 The characteristic absorption band of Si-OC bond is shown at 1090 cm-1. After sol-gel curing, the Si-OC bond in the Si-O-CH3 structure of castor oil-based polysiloxane is transformed into Si-O-Si bond, and its new absorption peak appears at 1090 cm-1. -1 This can well illustrate the successful synthesis of castor oil-based polysiloxane and the occurrence of sol-gel reaction; Figure 4 As shown, the MAHE in epoxidized soybean oil acrylate appears at 1638 cm -1 The peaks are the stretching vibration absorption peaks of the carbon-carbon double bond, among which 915cm -1 and 816cm -1 The infrared absorption peak of epoxy group is represented, indicating that epoxy soybean oil acrylate MAHE was successfully synthesized and has UV curing active double bonds.
[0087] 2. The photocurable films prepared in Examples 1-5 were tested for pencil hardness, adhesion, viscosity, curing shrinkage, curing time, resistance to waste water boiling and acid and alkali resistance. The test results are shown in Table 1:
[0088] (1) Pencil hardness test: The hardness of the photocurable film is tested according to the national standard GB / T6739 1996 (where pencil hardness 6H is the hardest, 6B is the softest, and the hardness range is 6B-HB-6H). The pencil hardness tester uses the three-point contact method to measure the surface of the cured film (where two points are rollers and one point is the pencil lead). The angle between the pencil and the surface of the cured film is 45°. Use the pencil hardness tester to slide on the surface of the cured film with a pressure of 1±0.05kg to observe the damage of the cured film. If no more than 2 damages occur in 5 tests, replace the hardness pencil of a higher grade for testing. If the cured film is damaged more than 2 times, the pencil grade can be read and the next grade of this grade can be recorded.
[0089] (2) Adhesion test: The test was conducted in accordance with ASTM D339-93B, where the sheet material was tinplate.
[0090] (3) Viscosity test: The photocured film was subjected to a shear rate-viscosity test using the MCR502 modular intelligent advanced rheometer produced by Anton Paar. The test standard was in accordance with GB / T2794-2013 “Determination of viscosity of adhesives”, and the viscosity of the cured film was recorded.
[0091] (4) Curing shrinkage: Determine the density of the photocurable material before and after curing. The density before curing is determined using the volume method. Total volume shrinkage = (density of sample after curing - density of sample before curing) / density of sample after curing × 100%. Record the measured curing shrinkage.
[0092] (5) Curing time: The curing time starts from when the UV lamp is turned on and stops when the surface of the curing material is dry. The curing time is recorded.
[0093] (6) Boiling water resistance test: A certain mass of the photocured film was placed in a boiling water bath at 100°C for 1 hour, then dried and weighed, and the changes before and after the boiling water bath were observed.
[0094] (7) Acid and alkali resistance test: A certain mass of photocured film was immersed in 10% hydrochloric acid and 10% sodium hydroxide for 48 hours, dried and weighed, and the changes before and after immersion were observed, and the performance results of the cured film were recorded.
[0095] Table 1 Performance test results of photocurable films
[0096]
[0097] The test results show that by continuously increasing the content of castor oil-based polysiloxane, the pencil hardness of the photocurable film will gradually increase to 4H, which indicates that the optimal ratio of castor oil-based polysiloxane to epoxidized vegetable oil-based acrylate can effectively improve the pencil hardness of the multifunctional vegetable oil-based silicone-containing acrylate photocurable film. In addition, the adhesion of the cured film can reach level 0, indicating that the cured film has good adhesion performance. At the same time, when used as a coating, the viscosity is relatively low and has good fluidity, ensuring that it can be well constructed. The prepolymer before curing has both a low curing shrinkage and a short curing time, indicating that the curing efficiency of the silicone-containing vegetable oil-based dual UV curing material is high, and it has a small curing shrinkage while being fast photocured. The photocurable film was boiled in boiling water, and the weight did not change after drying, indicating that the photocurable material has good resistance to boiling water. When the cured film was immersed in 10% HCL and 10% NAOH for 48 hours, there was no change in the HCL solution, but it could be completely dissolved in the 10% NAOH solution, which proved that the present invention has relatively good biodegradability and acid resistance.
[0098] 3. The mechanical properties of the photocured films prepared in Examples 1-4 were tested. The tensile properties of the photocured films were tested using a UTM5000 electronic universal testing machine. The crosshead speed was 10 mm / min and the sample size was 20 mm×10 mm×0.5 mm. The results are as follows:
[0099] The stress-strain curve of the multifunctional vegetable oil-based silicone-containing acrylate photocurable film is shown in Figure 5 , wherein R1-R4 are respectively Examples 1-4, Figure 5 It can be seen that the tensile strength of Example 4 is the largest, followed by Example 3, Example 2, and Example 1. It can be seen that adding silicon-containing ricinoleic acid-based acrylate to epoxy soybean oil acrylate can effectively enhance the tensile strength, and it can be seen from the test results that when the ratio of castor oil-based polysiloxane to epoxidized vegetable oil-based acrylate is 4:1, the tensile strength reaches the strongest. This is mainly due to the increase in the ratio of castor oil-based polysiloxane, which causes the ratio of flexible chains to gradually increase. Therefore, the tensile strength of Example 4 is smaller than that of Example 1. Although the elongation at break is smaller than that of Example 1, the gap is not large, indicating that the ratio of castor oil-based polysiloxane to epoxidized vegetable oil-based acrylate in Example 4 takes into account both tensile strength and elongation at break. In addition, it is explained that the increase of castor oil-based polysiloxane can well improve the tensile strength, and the photopolymerization cross-linking reaction of the three groups of carbon-carbon double bonds, epoxy groups and methoxysilane has a synergistic effect with the three cross-linking methods, which can further improve the cross-linking degree of the reaction system. The present invention can obtain light-curable materials with different properties by adjusting the ratio of castor oil-based polysiloxane and epoxidized vegetable oil-based acrylate, so as to adapt to applications in different environments.
[0100] 4. The photocured films prepared in Examples 1-4 were subjected to a shear rate-viscosity test using the MCR502 modular intelligent advanced rheometer from Anton Paar. The test standard was in accordance with GB / T2794-2013 "Determination of viscosity of adhesives". The results are as follows:
[0101] Shear rate-viscosity of multifunctional vegetable oil-based silicone-containing acrylate photocurable film Figure 6 As the amount of castor oil-based polysiloxane increases, the viscosity decreases. This is because the Si-O-Si bonds in the curing material gradually increase, the flexible chains increase, and the viscosity decreases accordingly, making the liquid material before light curing have better leveling properties. In addition, the viscosity does not change with the increase in shear rate, indicating that it is a Newtonian fluid. When used as a coating, the viscosity is relatively low and has good fluidity, ensuring that it can be well constructed.
[0102] 5. The storage modulus (E') and loss factor (tan δ) of the photocured films obtained in Examples 1-5 were tested. The test instrument used a DMA242C dynamic mechanical analyzer from Netzsch, Germany. The sample holder used a tensile holder. The oscillation frequency was 1 Hz. The sample size was 20 mm × 6 mm × 0.5 mm. The heating rate was 3 °C / min. The temperature range was -80 to 180 °C. The crosslinking density v was calculated according to the rubber elastic dynamics theory. e , see the following formula, where E' is the storage modulus at Tg+30°C, R is the gas constant, and T is the absolute temperature of the photocurable material at Tg+30°C:
[0103]
[0104] The results are as follows:
[0105] Storage modulus (E') and loss factor (tanδ) of multifunctional vegetable oil-based silicone-containing acrylate photocurable films as a function of temperature Figure 7 and Figure 8 As shown, the loss factor is the same as the glass transition temperature value Tg. As the castor oil-based polysiloxane increases, the elastic fatty chains increase and the rigid fatty rings decrease, resulting in a decrease in the glass transition temperature. And as the castor oil-based polysiloxane increases, the chain-chain interaction of the long-chain fatty acids leads to the relative migration of the network. The combination of these properties leads to a looser network, which exhibits additional fluidity and ultimately reduces Tg. The final results are shown in Table 2.
[0106] Table 2 Storage modulus and glass transition temperature test results
[0107]
[0108]
[0109] 6. After coating the pattern surface with Example 1, Example 3 and Example 4, digital macroscopic morphology observation was performed, where R0 is the image of the covered glass plate, and the results are as follows:
[0110] The transparency of multifunctional vegetable oil-based silicone-containing acrylate photocurable film is shown in Fig. 9 ,Compared with the transparent glass plate, the silicone plant oil based double UV curing material is light yellow, and the overall transparency of the film is good.
[0111] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing a silicon-containing vegetable oil-based dual UV curing material, characterized in that: The following steps are involved: Step (1), preparation of castor oil-based polysiloxane: stir ricinoleic acid, acid anhydride and catalyst at 75-95° C. in a nitrogen atmosphere for 2-4 hours, add silane coupling agent KH-560 and polymerization inhibitor to continue reaction, and obtain castor oil-based polysiloxane; Step (2), preparation of epoxidized vegetable oil-based acrylate: stirring hydroxyethyl acrylate, acid anhydride and catalyst at 75-95° C. for 2-4 hours, adding epoxidized vegetable oil and inhibitor to continue the reaction, and obtaining epoxidized vegetable oil-based acrylate; Step (3), mixing castor oil-based polysiloxane with epoxidized vegetable oil-based acrylate, adding a composite photoinitiator and a reactive diluent and mixing evenly to obtain a silicon-containing vegetable oil-based dual UV curing material; The composite photoinitiator includes a free radical photoinitiator and a cationic photoinitiator.
2. The method for preparing the silicon-containing vegetable oil-based dual UV curing material according to claim 1, characterized in that: In the step (3), according to the mass percentage of the total mass of the raw materials of castor oil-based polysiloxane, epoxidized vegetable oil-based acrylate, composite photoinitiator and reactive diluent, 10-60% of castor oil-based polysiloxane and 10-60% of epoxidized vegetable oil-based acrylate are mixed, and 1-10% of the composite photoinitiator and 10-50% of the reactive diluent are added and mixed evenly to obtain a silicon-containing vegetable oil-based dual UV curing material.
3. The method for preparing the silicon-containing vegetable oil-based dual UV curing material according to claim 1, characterized in that: In the step (3), the mass ratio of castor oil-based polysiloxane to epoxidized vegetable oil-based acrylate is (1-4): (1-4).
4. The method for preparing the silicon-containing vegetable oil-based dual UV curing material according to claim 1, characterized in that: In the step (1), ricinoleic acid, anhydride and a catalyst are stirred at 75 to 95° C. in a nitrogen atmosphere for 2 to 4 hours, a silane coupling agent KH-560 and a polymerization inhibitor are added, and the catalyst is added and then the reaction is continued, and the mixture is stirred at 70 to 90° C. for 5 to 12 hours to obtain a castor oil-based polysiloxane; In the step (1), the molar ratio of the ricinoleic acid, the acid anhydride and the silane coupling agent KH-560 is 1: (1-2.5): (1-2.5), the total amount of the catalyst added is 0.4-2% of the total mass of the ricinoleic acid, the acid anhydride and the silane coupling agent KH-560, and the amount of the inhibitor added is 0.01-1% of the total mass of the ricinoleic acid, the acid anhydride and the silane coupling agent KH-560.
5. The method for preparing the silicon-containing vegetable oil-based dual UV curing material according to claim 1, characterized in that: In the step (2), hydroxyethyl acrylate, acid anhydride and catalyst are stirred at 75-95°C for 2-4 hours, epoxidized vegetable oil and inhibitor are added, and the catalyst is added and the reaction is continued, and the reaction is stirred at 75-95°C for 4-6 hours to obtain epoxidized vegetable oil-based acrylate; In the step (2), the molar ratio of the epoxidized vegetable oil, the acid anhydride and the hydroxyethyl acrylate is 1:(1-2.5):(1-2.5), the total amount of the catalyst added is 0.5-2.5% of the total mass of the epoxidized vegetable oil, the acid anhydride and the hydroxyethyl acrylate, and the amount of the inhibitor added is 0.01-0.08% of the total mass of the epoxidized vegetable oil, the acid anhydride and the hydroxyethyl acrylate.
6. The method for preparing the silicon-containing vegetable oil-based dual UV curing material according to claim 1, characterized in that: In the step (2), the epoxidized vegetable oil is any one or more of epoxidized rapeseed oil, epoxidized castor oil, epoxidized palm oil and epoxidized soybean oil; In the step (1) and the step (2), the acid anhydride is any one or more of a combination of maleic anhydride, succinic anhydride and phthalic anhydride, the catalyst is any one or more of a combination of N,N-dimethylbenzylamine, triethylamine, tetrabutylammonium bromide and triphenylphosphine, and the inhibitor is any one or more of a combination of hydroquinone, 4-methoxyphenol, 2,5-di-tert-butyl-p-cresol and tert-butylhydroquinone.
7. The method for preparing the silicon-containing vegetable oil-based dual UV curing material according to claim 1, characterized in that: In the step (3), the composite photoinitiator is composed of a free radical photoinitiator and a cationic photoinitiator, and the mass ratio of the free radical photoinitiator to the cationic photoinitiator is (1-9): (1-9); The free radical photoinitiator is any one or more combinations of 2-hydroxy-2-methyl-phenylacetone-1, 1-hydroxy-cyclohexyl benzophenone, 2-hydroxy-2-methyl-p-hydroxyethyl ether phenylacetone-1, 2-methyl-1-(4-methylthiophenyl)-2-morpholinyl-1-propanone, 2,4,6-trimethylbenzoyl-ethoxy-phenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide and 4-p-toluenethiodibenzophenone, and the cationic photoinitiator is any one or more combinations of diazonium salts, diaryliodonium salts, triarylsulfonium salts, alkylsulfonium salts, iron arene salts, sulfonyloxy ketones and triarylsiloxane ethers.
8. The method for preparing the silicon-containing vegetable oil-based dual UV curing material according to claim 1, characterized in that: In the step (3), the active diluent is any one or more of tripropylene glycol diacrylate, 1,6-hexanediol diacrylate, glycidyl acrylate and glycidyl methacrylate.
9. A silicon-containing vegetable oil-based dual UV curing material, characterized in that: The silicon-containing vegetable oil-based dual UV curing material is prepared by the preparation method of any one of claims 1 to 8.