A polyamide material containing pentaphenylamine in the main chain and its preparation method and application

By designing an electroactive polyamide material containing pentaaniline in the main chain, the problem of solubility and processing capability of polyaniline in industrial applications has been solved, and the efficient optical performance and long-term cycle stability of electrochromic capacitive windows have been achieved, which can regulate indoor light. and solar radiation, and achieve energy storage and reuse.

CN116655909BActive Publication Date: 2024-10-29JILIN UNIVERSITY
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310645945.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-02
Publication Date
2024-10-29
Estimated Expiration
2043-06-02

AI Technical Summary

Technical Problem

Existing polyaniline materials have poor solubility and processing capabilities in industrial applications, and are prone to corrosion of indium tin oxide current collectors during the electrochemical process, resulting in insufficient long-term cycle durability of electrochromic supercapacitors and inability to effectively modulate indoor temperature and lighting levels.

Method used

Design an electroactive polyamide material containing pentaphenylamine in the main chain, prepare the easy-to-process polyamide through a specific synthesis method, and apply it in the electrochromic capacitor window, combined with the V2O5/ITO counter electrode and gel electrolyte to form Sandwich-structured electrochromic capacitive window.

Benefits of technology

It achieves good solubility and optical properties of polyamide materials, has fast response and long-term cycle stability, can regulate light and solar radiation, realize energy storage and reuse, and reduce energy loss.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116655909B_ABST
    Figure CN116655909B_ABST
Patent Text Reader

Abstract

The present invention relates to a polyamide material containing pentaphenylamine in the main chain, and a preparation method and application thereof. The purpose of the present invention is to solve the problems that the polyaniline prepared by the existing method is not easy to process, has poor stability, and ordinary windows cannot modulate the indoor temperature and lighting level. The preparation method of the polyamide material containing pentaphenylamine in the main chain of the present invention comprises: designing and synthesizing an electroactive amide monomer; designing and synthesizing an electroactive polyamide EPA; preparing an EPA working electrode, a vanadium pentoxide counter electrode and a gel electrolyte; and assembling an electrochromic capacitor window. The preparation method of the polyamide material containing pentaphenylamine in the main chain of the present invention obtains a new type of electroactive polyamide, which is not only convenient to process, but also has electrochromic and energy storage properties; the method for synthesizing polyamide of the present invention is simple and can be mass-produced; the electrochromic capacitor window assembled by the preparation method of the present invention can simultaneously adjust the room temperature and lighting level, and can also store energy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of conductive functional polymers, and specifically relates to an electroactive polyamide material containing pentaphenylamine on the main chain, a preparation method thereof, and application of the material in an electrochromic capacitor window. Background Art

[0002] Electrochromic supercapacitors have become very popular in recent years due to their ability to possess both electrochromic and energy storage properties. Polyaniline has been widely studied for the fabrication of electrochromic supercapacitor devices due to its significant advantages, such as high theoretical capacitance, reversible electrochemical activity, large optical contrast, and fast redox conversion rate. However, due to chain rigidity and strong interchain interactions, the solubility and processing ability of polyaniline are extremely poor, which seriously affects the industrial application of polyaniline. At the same time, the common electrolyte in the electrochemical process is acidic, which can severely corrode the indium tin oxide (ITO) collector. On the other hand, the continuous insertion and deinsertion of small molecule dopants can lead to repeated expansion and contraction of the polyaniline film, causing the functional layer to break or collapse. The long-term cycle durability of electrochromic supercapacitors has not yet reached the benchmark for practical application. Summary of the invention

[0003] The purpose of the present invention is to address the deficiencies of the above-mentioned prior art and to provide a novel polyamide material containing pentaphenylamine on the main chain, a preparation method and its application in electrochromic capacitor windows, so as to solve the problems that the polyaniline prepared by the existing method is not easy to process and has poor stability, and that ordinary windows cannot modulate indoor temperature and lighting levels.

[0004] The objective of the present invention is achieved through the following technical solutions:

[0005] An electroactive polyamide EPA containing pentaphenylamine in the main chain, wherein the polyamide has a repeating unit of the structure shown in formula (I):

[0006]

[0007] Furthermore, the amide monomer EA in the structure of formula (I) has a structure shown in formula (II):

[0008]

[0009] A method for preparing an electroactive polyamide EPA containing pentaphenylamine in the main chain, the steps of which are as follows:

[0010] A. Synthesis of electroactive amide monomer EA:

[0011] A1. Place 2.58-5.15 g, 14-28 mmol, of p-aminodiphenylamine and 30 mL of dry DMF solution in a reaction vessel, and perform ultrasonic treatment for 15 minutes;

[0012] A2, dissolve 1.02-2.04 g, 5-10 mmol, of terephthaloyl chloride in 20 mL of DMF;

[0013] A3, dropwise adding the DMF solution of terephthaloyl chloride into the DMF solution of p-aminodiphenylamine, and reacting for 6 hours;

[0014] A4. Pour the mixed solution into 300 mL of ice water for precipitation, and wash the resulting precipitate with distilled water, ethanol, dichloromethane and ether in sequence;

[0015] A5, dried under vacuum at 45°C for 24 hours to obtain gray-green solid EA;

[0016] B. Synthesis of electroactive polyamide EPA:

[0017] B1. Add 1.00-2.00 g, 2-4 mmol, of EA and 0.228-0.456 g, 2.1-4.2 mmol, of p-phenylenediamine into a reaction vessel, and pour in 40 mL of DMF solution;

[0018] B2. During the stirring process, 15 mL of 3 mol / L hydrochloric acid solution was added dropwise to the above DMF solution to form a uniform dispersion;

[0019] B3, transfer 0.92-1.84 g, 4-8 mmol of ammonium persulfate into 10 mL, 3 mol / L hydrochloric acid;

[0020] B4, adding the hydrochloric acid solution of ammonium persulfate dropwise to the above dispersion for 30 minutes, and reacting at room temperature for 24 hours;

[0021] B5. Pour the reaction mixture into 300 mL of ice water for precipitation, filter the precipitate, and wash with distilled water, ethanol and acetone in sequence until it is colorless;

[0022] B6. Disperse the precipitate with a 2.5 mol / L ammonia solution, reduce it with hydrazine hydrate in a molar amount of 6 times that of the amide monomer EA, and then transfer it to a 45° C. vacuum oven and dry it for 24 hours to obtain dark green solid EPA.

[0023] Furthermore, in step A, the molar ratio of p-aminodiphenylamine to terephthaloyl chloride is 2.8:1.

[0024] Furthermore, in step B, the molar ratio of EA, terephthaloyl chloride and ammonium persulfate is 1:1.05:2.

[0025] Furthermore, in step B6, the molar ratio of the amide monomer EA to the hydrazine hydrate is 1:6.

[0026] Application of an electroactive polyamide EPA containing pentaphenylamine in the main chain in an electrochromic capacitor window, the capacitor window assembly steps are as follows:

[0027] C. Preparation of EPA / ITO working electrode, V 2 O 5 / ITO counter electrode and gel electrolyte;

[0028] D. Place the gel electrolyte between the EPA / ITO working electrode and V 2 O 5 / ITO counter electrodes form a sandwich structure;

[0029] E. Use photocuring adhesive to stick the copper tape to the positive and negative poles of the device to obtain an electrochromic capacitor window.

[0030] Furthermore, in step C, the EPA / ITO working electrode preparation method is as follows:

[0031] C1. Dissolve 10-12 mg EPA in 1 mL DMF to prepare a uniform solution.

[0032] C2, drop the EPA DMF solution onto the ITO glass substrate and spin coat at 3000 r / min for 30 seconds to form a uniform film;

[0033] C3. The ITO glass substrate with the uniform thin film was transferred to a vacuum oven at 45° C. and dried for 24 hours to obtain an EPA / ITO working electrode.

[0034] Furthermore, in step C, V 2 O 5 / ITO counter electrode preparation method is as follows:

[0035] C4, at 60°C, 1.0-1.2g of V 2 O 5 and 1.2-1.44 g of NaCl in 100 mL of deionized water and stirred for 36 hours until a color change from yellow to brown occurred;

[0036] C5. Centrifuge the mixture at 6000 r / min for three times, rinse with deionized water and ethanol until colorless, and collect the precipitate;

[0037] C6. The above precipitate was transferred to a vacuum oven at 45°C and dried for 24 hours to obtain V 2 O 5 Nanowires;

[0038] C7, 2 mg of V 2 O 5 The nanowires were uniformly dispersed in 5 mL of deionized water.2 O 5 The nanowire solution was spin-coated at 2000 r / min for 30 s to form a uniform film;

[0039] C8, annealed at 60°C for 1 hour, obtained V 2 O 5 / ITO counter electrode.

[0040] Furthermore, in step C4, V 2 O 5 / ITO counter electrode preparation process 2 O 5 The mass ratio of NaCl is 1:1.2.

[0041] Compared with the prior art, the present invention has the following beneficial effects:

[0042] 1. The polyamide material containing pentaphenylamine in the main chain designed by the present invention has good solubility, is easy to process, has excellent optical properties, fast response speed, good open circuit memory ability, large capacitance and long-term charge and discharge cycle stability;

[0043] 2. The synthetic method designed by the present invention is simple to operate and has low raw material cost, which is conducive to the industrial production of the electroactive polyamide material;

[0044] 3. The electrochromic capacitor window assembled by the present invention has both electrochromic and energy storage properties. It adjusts the light and solar radiation in the building by adjusting its own optical transmittance, thereby achieving simultaneous adjustment of room temperature and lighting level. At the same time, the stored energy can also be released to achieve energy recovery and reuse. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on the provided drawings without creative work.

[0046] Figure 1 The electroactive amide monomer EA synthesized by the present invention is 1 H NMR spectra;

[0047] Figure 2 FTIR graph of the electroactive amide monomer EA synthesized in the present invention;

[0048] Figure 3 The electroactive polyamide EPA synthesized by the present invention 1 H NMR spectra;

[0049] Figure 4 FTIR graph of the electroactive polyamide EPA synthesized in the present invention;

[0050] Figure 5 is a TGA curve diagram of the electroactive polyamide EPA synthesized by the present invention;

[0051] Figure 6 The EPA / ITO working electrode prepared from the electroactive polyamide EPA synthesized by the present invention is in the three-electrode (0.1MLiClO 4 / acetonitrile as electrolyte, EPA / ITO as working electrode, Ag / Ag + CV curves of different scan rates tested in a system with a Pt electrode as the reference electrode and a Pt wire as the counter electrode;

[0052] Figure 7 The transmittance variation curve of the EPA / ITO working electrode prepared by the present invention at a voltage of -0.5 to 1V;

[0053] Figure 8 V prepared by the present invention 2 O 5 / SEM image of ITO counter electrode;

[0054] Fig. 9 The EPA / ITO working electrode, gel electrolyte and V 2 O 5 CV curves of the electrochromic capacitor window assembled with electrodes at different scanning rates;

[0055] Fig.10 The transmittance variation curve of the electrochromic capacitor window assembled by the present invention at 0V and 2V voltages;

[0056] Fig.11 The transmittance change and response time diagram of the electrochromic capacitor window assembled by the present invention under a square wave voltage in the visible light range;

[0057] Fig.12 The transmittance change and response time diagram of the electrochromic capacitive window assembled by the present invention under a square wave voltage in the near infrared range;

[0058] Fig.13 The stable performance diagram of the electrochromic capacitor window assembled by the present invention during 10,000 long cycle charge and discharge processes;

[0059] Fig.14 Synthesis route of electroactive polyamide EPA containing pentaphenylamine as the main chain. DETAILED DESCRIPTION

[0060] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. It is to be understood that the specific embodiments described herein are only used to explain the present invention, rather than to limit the present invention. It should also be noted that, for ease of description, only parts related to the present invention, rather than all structures, are shown in the accompanying drawings.

[0061] The polyamide designed by the present invention is soluble in common organic solvents such as N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), dimethyl sulfoxide (DMSO), etc., so as to carry out solvent processing. In addition, the polyamide can maintain high activity and electrochemical stability in non-acidic electrolytes. The electrochromic capacitor window is composed of an electrochromic supercapacitor containing polyamide, which adjusts the optical transmittance by electrochemically regulating its redox state, so that the light and solar radiation in the building can be adjusted as needed, which realizes the simultaneous regulation of room temperature and lighting level. At the same time, the stored energy can also be released for the operation of household appliances, realizing energy recovery and reuse, and greatly reducing energy loss.

[0062] The present invention designs and synthesizes a processable polyamide (EPA) containing pentaphenylamine on the main chain through oxidative coupling polymerization. The optical properties, response speed, open circuit memory ability, electrochemical properties and cycle stability of EPA are studied in detail. Then, an electrochromic capacitor window with both electrochromic and energy storage properties is made with EPA, showing excellent indoor regulation and energy storage properties. This shows the reasonable design ideas of EPA molecules and the satisfactory electrochromic and pseudocapacitive properties, which provides the possibility for the preparation of the next generation of electrochromic capacitor windows and contributes to the realization of green buildings.

[0063] Specific implementation 1: This implementation includes a polyamide material containing pentaphenylamine in the main chain and a preparation method and application thereof, which are completed according to the following steps:

[0064] The preparation method of the electroactive polyamide EPA containing pentaphenylamine in the main chain of the present invention comprises the following steps:

[0065] Step 1: Synthesis of electroactive amide monomer EA:

[0066] ①, Place 2.58-4.41 g (14-21 mmol) of p-aminodiphenylamine and 30 mL of dry N,N-dimethylformamide (DMF) solution in a 100 mL round-bottom flask, and perform ultrasonic treatment for 15 minutes;

[0067] ②, dissolve terephthaloyl chloride (1.02-1.53 ​​g, 5-7.5 mmol) in 20 mL DMF;

[0068] ③, drop the DMF solution of terephthaloyl chloride into the DMF solution of p-aminodiphenylamine, and react for 6 hours;

[0069] ④. Pour the mixed solution into 300 mL of ice water to obtain a precipitate, and rinse it with distilled water, ethanol, dichloromethane and ether in sequence;

[0070] ⑤. Dry under vacuum at 45°C for 24 hours to obtain gray-green solid EA.

[0071] Step 2: Synthesis of electroactive polyamide EPA:

[0072] ①, add 1.00-1.50 g (2-3 mmol) EA and 0.228-0.342 g (2.1-3.15 mmol) p-phenylenediamine into a 100 mL round-bottom flask, and pour in 40 mL of DMF solution;

[0073] ②, during the stirring process, add 15mL of 3mol / L hydrochloric acid solution dropwise to the above DMF solution to form a uniform dispersion;

[0074] ③. Transfer 0.92-1.38 g (4-6 mmol) of ammonium persulfate into 10 mL of 3 mol / L hydrochloric acid;

[0075] ④. Add the hydrochloric acid solution of ammonium persulfate to the above dispersion for 30 minutes. The reaction is carried out at room temperature for 24 hours;

[0076] ⑤. Pour the reaction mixture into 300 mL of ice water and precipitate. Filter the precipitate and wash with distilled water, ethanol and acetone in sequence until it is colorless;

[0077] ⑥. Disperse the precipitate with a 2.5 mol / L ammonia solution, reduce it with hydrazine hydrate in a molar amount of 6 times that of the amide monomer EA, and then transfer it to a 45°C vacuum oven and dry it for 24 hours to obtain dark green solid EPA.

[0078] Furthermore, the electroactive polyamide EPA described in the present invention is used in an electrochromic capacitor window, and the capacitor window assembly steps are as follows:

[0079] Step 1: Preparation of EPA / indium tin oxide (ITO) working electrode, vanadium pentoxide (V 2 O 5 ) / ITO counter electrode and gel electrolyte.

[0080] Step 2: Place the gel electrolyte between the EPA / ITO working electrode and V 2 O 5 / ITO counter electrodes form a sandwich structure.

[0081] Step 3: Use photocuring adhesive to stick the copper tape to the positive and negative poles of the device to obtain the electrochromic capacitor window.

[0082] The preparation method of the EPA / ITO working electrode in step 1 is as follows:

[0083] ① Dissolve 10-11 mg EPA in 1 mL DMF to prepare a uniform solution;

[0084] ②, drop the EPA DMF solution onto the ITO glass substrate and spin coat at 3000r / min for 30 seconds to form a uniform film;

[0085] ③. Transfer the above-mentioned ITO glass substrate with a uniform thin film to a vacuum oven at 45° C. and dry it for 24 hours to obtain an EPA / ITO working electrode.

[0086] In step 1, V 2 O 5 The preparation method of ITO counter electrode is as follows:

[0087] ①, at 60℃, V 2 O 5 (1.0-1.1 g) and NaCl (1.2-1.32 g) were stirred in 100 mL of deionized water for 36 h until a color change from yellow to brown occurred;

[0088] ② Centrifuge the mixture at 6000r / min three times, rinse with deionized water and ethanol until colorless, and collect the precipitate;

[0089] ③. The above precipitate was transferred to a vacuum oven at 45°C and dried for 24 hours to obtain V 2 O 5 Nanowires;

[0090] ④, 2 mg of V 2 O 5 The nanowires were uniformly dispersed in 5 mL of deionized water. 2 O 5 The nanowire solution was spin-coated at 2000 r / min for 30 s to form a uniform film;

[0091] ⑤, anneal at 60℃ for 1 hour to obtain V 2 O 5 / ITO counter electrode.

[0092] Specific embodiment 2: This embodiment differs from specific embodiment 1 in that the amount of p-aminodiphenylamine in step 1 of the preparation method of electroactive polyamide EPA is 3.68-4.29 g (17.5-23.3 mmol), and the amount of terephthaloyl chloride is (1.28-1.7 g, 6.25-8.33 mmol). The other steps are the same as those in specific embodiment 1.

[0093] Specific embodiment 3: This embodiment differs from specific embodiment 1 or 2 in that: in step 1 of the preparation method of electroactive polyamide EPA, the amount of p-aminodiphenylamine is 4.41-5.15 g (21-28 mmol), and the amount of terephthaloyl chloride is (1.53-2.04 g, 7.5-10 mmol). The other steps are the same as those of specific embodiment 1 or 2.

[0094] Specific embodiment 4: This embodiment differs from any one of specific embodiments 1 to 3 in that the amount of EA in step 2 of the preparation method of electroactive polyamide EPA is 1.25 to 1.67 g (2.5 to 3.33 mmol), the amount of p-phenylenediamine is 0.285 to 0.38 g (2.63 to 3.5 mmol), and the amount of ammonium persulfate is 1.15 to 1.53 g (5 to 6.67 mmol). The other steps are the same as those of specific embodiments 1 to 3.

[0095] Specific embodiment 5: This embodiment differs from any one of specific embodiments 1 to 4 in that the amount of EA in step 2 of the preparation method of electroactive polyamide EPA is 1.50 to 2.00 g (3 to 4 mmol), the amount of p-phenylenediamine is 0.342 to 0.456 g (3.15 to 4.2 mmol), and the amount of ammonium persulfate is 1.38 to 1.84 g (6 to 8 mmol). The other steps are the same as those of specific embodiments 1 to 4.

[0096] Specific embodiment 6: This embodiment differs from any one of specific embodiments 1 to 5 in that: during the assembly of the capacitive window, the EPA / ITO working electrode in step 1 is prepared by dissolving 11-12 mg EPA in 1 mL DMF. The other steps are the same as those in specific embodiments 1 to 5.

[0097] Specific implementation 7: This implementation differs from any one of specific implementations 1 to 6 in that: during the capacitor window assembly process, the V 2 O 5 / ITO counter electrode preparation V 2 O 5 The amount of is 1.1-1.2 g, and the amount of NaCl is 1.32-1.44 g. The other steps are the same as those in Specific Embodiments 1 to 6.

[0098] The following examples are used to verify the beneficial effects of the present invention:

[0099] Example 1: Preparation method of electroactive amide monomer EA.

[0100] ①, Place 2.58 g (14 mmol) of p-aminodiphenylamine and 30 mL of dry N,N-dimethylformamide (DMF) solution in a 100 mL round-bottom flask, and perform ultrasonic treatment for 15 minutes;

[0101] ②, dissolve terephthaloyl chloride (1.02 g, 5 mmol) in 20 mL DMF;

[0102] ③, drop the DMF solution of terephthaloyl chloride into the DMF solution of p-aminodiphenylamine, and react for 6 hours;

[0103] ④. Pour the mixed solution into 300 mL of ice water to obtain a precipitate, and rinse it with distilled water, ethanol, dichloromethane and ether in sequence;

[0104] ⑤. Dry under vacuum at 45°C for 24 hours to obtain gray-green solid EA.

[0105] Example 2: Preparation method of electroactive amide monomer EA.

[0106] ①, Place 5.15 g (28 mmol) of p-aminodiphenylamine and 30 mL of dry N,N-dimethylformamide (DMF) solution in a 100 mL round-bottom flask, and treat with ultrasound for 15 minutes;

[0107] ②, dissolve terephthaloyl chloride (2.04 g, 10 mmol) in 20 mL DMF;

[0108] ③, drop the DMF solution of terephthaloyl chloride into the DMF solution of p-aminodiphenylamine, and react for 6 hours;

[0109] ④. Pour the mixed solution into 300 mL of ice water to obtain a precipitate, and rinse it with distilled water, ethanol, dichloromethane and ether in sequence;

[0110] ⑤. Dry under vacuum at 45°C for 24 hours to obtain gray-green solid EA.

[0111] Figure 1 and Figure 2 This is a structural representation diagram of the electroactive amide monomer EA synthesized in the present invention. Figure 1 For the synthesis of electroactive amide monomer EA 1 In the H NMR diagram, the characteristic signals of -CONH- and -NH- are located at 10.27 ppm and 7.66 ppm respectively. The remaining hydrogen is aromatic hydrogen and is located between 6 ppm and 9 ppm.

[0112] Figure 2 The FTIR spectrum of the synthesized electroactive amide monomer EA. The stretching vibrations of amide and amine appear at 3398 cm -1 、3370cm -1 and 3303cm -1 The absorption peak of CH stretching vibration of benzene ring appears at 3042cm -1 . At 1650-1450cm -1 The absorption in the range should be attributed to the C=C stretching vibration on the benzene ring. As polyamide, EA has a peak at 1704 cm -1 and 1311cm -1 The characteristic C=O and CN stretching vibration peaks are shown at .

[0113] Example 3: Preparation method of electroactive polyamide EPA.

[0114] ①, add 1.00 g (2 mmol) EA and 0.228 g (2.1 mmol) p-phenylenediamine into a 100 mL round-bottom flask, and pour in 40 mL of DMF solution;

[0115] ②, during the stirring process, add 15mL of 3mol / L hydrochloric acid solution dropwise to the above DMF solution to form a uniform dispersion;

[0116] ③. Transfer 0.92 g (4 mmol) of ammonium persulfate into 10 mL of 3 mol / L hydrochloric acid;

[0117] ④. Add the hydrochloric acid solution of ammonium persulfate to the above dispersion for 30 minutes. The reaction is carried out at room temperature for 24 hours;

[0118] ⑤. Pour the reaction mixture into 300 mL of ice water and precipitate. Filter the precipitate and wash with distilled water, ethanol and acetone in sequence until it is colorless;

[0119] ⑥. Disperse the precipitate with a 2.5 mol / L ammonia solution, reduce it with hydrazine hydrate in a molar amount of 6 times the amide monomer EA, and then transfer it to a 45°C vacuum oven and dry it for 24 hours to obtain dark green solid EPA.

[0120] Example 4: Preparation method of electroactive polyamide EPA.

[0121] ①, add 1.50g (3mmol) EA and 0.342g (3.15mmol) p-phenylenediamine into a 100mL round-bottom flask, and pour in 40mL DMF solution;

[0122] ②, during the stirring process, add 15mL 3mol / L hydrochloric acid solution dropwise to the above DMF solution to form a uniform dispersion;

[0123] ③. Transfer 1.38 g (6 mmol) of ammonium persulfate into 10 mL of 3 mol / L hydrochloric acid;

[0124] ④. Add the hydrochloric acid solution of ammonium persulfate to the above dispersion for 30 minutes. The reaction is carried out at room temperature for 24 hours;

[0125] ⑤. Pour the reaction mixture into 300 mL of ice water and precipitate. Filter the precipitate and wash with distilled water, ethanol and acetone in sequence until it is colorless;

[0126] ⑥. Disperse the precipitate with a 2.5 mol / L ammonia solution, reduce it with hydrazine hydrate in a molar amount of 6 times that of the amide monomer EA, and then transfer it to a 45°C vacuum oven and dry it for 24 hours to obtain dark green solid EPA.

[0127] Example 5: Preparation method of electroactive polyamide EPA.

[0128] ①, add 2.00g (4mmol) EA and 0.456g (4.2mmol) p-phenylenediamine into a 100mL round-bottom flask, and pour in 40mL DMF solution;

[0129] ②, during the stirring process, add 15mL 3mol / L hydrochloric acid solution dropwise to the above DMF solution to form a uniform dispersion;

[0130] ③. Transfer 1.84 g (8 mmol) of ammonium persulfate into 10 mL of 3 mol / L hydrochloric acid;

[0131] ④. Add the hydrochloric acid solution of ammonium persulfate to the above dispersion for 30 minutes. The reaction is carried out at room temperature for 24 hours;

[0132] ⑤. Pour the reaction mixture into 300 mL of ice water and precipitate. Filter the precipitate and wash with distilled water, ethanol and acetone in sequence until it is colorless;

[0133] ⑥. Disperse the precipitate with a 2.5 mol / L ammonia solution, reduce it with hydrazine hydrate in a molar amount of 6 times that of the amide monomer EA, and then transfer it to a 45°C vacuum oven and dry it for 24 hours to obtain dark green solid EPA.

[0134] Figure 3 For the synthesis of electroactive polyamide EPA 1 H NMR spectrum. The characteristic signals of -CONH- and -NH- are located near 10.28 ppm and 7.58 ppm respectively. The remaining hydrogen is aromatic hydrogen and is located between 5 ppm and 10 ppm.

[0135] Figure 4FTIR spectrum of the synthesized electroactive polyamide EPA. The stretching vibrations of amide and amine appear at 3394 cm -1 、3367cm -1 and 3299cm -1 The absorption peak of CH stretching vibration of benzene ring appears at 3035cm -1 . At 1650-1450cm -1 The absorption in the range is attributed to the C=C stretching vibration on the benzene ring. As a polyamide, EPA has a wavelength of 1700 cm -1 and 1303cm -1 The characteristic C=O and CN stretching vibration peaks are shown at .

[0136] Figure 5 The TGA curve of the synthesized electroactive polyamide EPA is shown in Figure 2. The thermal stability of EPA was investigated by TGA test in a nitrogen environment. The intersection temperature of the baseline and the tangent line of the thermogravimetric curve at the maximum slope is defined as the initial decomposition temperature (T d ), the temperature at which the compound loses 5% of its mass is T 5%loss The TGA curve shows that the T d 192℃, T 5%loss It is 279℃, which shows that EPA has relatively good thermodynamic stability, providing safety for its application in high temperature environment.

[0137] Example 6: Application of electroactive polyamide EPA in electrochromic capacitor window.

[0138] Step 1: Preparation of EPA / ITO working electrode, vanadium pentoxide (V 2 O 5 ) / ITO counter electrode and gel electrolyte.

[0139] Step 2: Place the gel electrolyte between the EPA / ITO working electrode and V 2 O 5 / ITO counter electrodes form a sandwich structure.

[0140] Step 3: Use photocuring adhesive to stick the copper tape to the positive and negative poles of the device to obtain the electrochromic capacitor window.

[0141] The preparation method of the EPA / ITO working electrode described in step 1 is as follows:

[0142] ① Dissolve 10 mg EPA in 1 mL DMF to prepare a uniform solution;

[0143] ②, drop the EPA DMF solution onto the ITO glass substrate and spin coat at 3000r / min for 30 seconds to form a uniform film;

[0144] ③. Transfer the above-mentioned ITO glass substrate with a uniform thin film to a vacuum oven at 45° C. and dry it for 24 hours to obtain an EPA / ITO working electrode.

[0145] Step 1 V 2 O 5 / ITO counter electrode preparation method is as follows:

[0146] ①, at 60℃, V 2 O 5 (1.0 g) and NaCl (1.2 g) were stirred in 100 mL of deionized water for 36 h until a color transition from yellow to brown occurred;

[0147] ② Centrifuge the mixture at 6000r / min three times, rinse with deionized water and ethanol until colorless, and collect the precipitate;

[0148] ③. The above precipitate was transferred to a vacuum oven at 45°C and dried for 24 hours to obtain V 2 O 5 Nanowires;

[0149] ④, 2 mg of V 2 O 5 The nanowires were uniformly dispersed in 5 mL of deionized water. 2 O 5 The nanowire solution was spin-coated at 2000 r / min for 30 s to form a uniform film;

[0150] ⑤, anneal at 60℃ for 1 hour to obtain V 2 O 5 / ITO counter electrode.

[0151] Example 7: Application of electroactive polyamide EPA in electrochromic capacitor window.

[0152] Step 1: Preparation of EPA / ITO working electrode, vanadium pentoxide (V 2 O 5 ) / ITO counter electrode and gel electrolyte.

[0153] Step 2: Place the gel electrolyte between the EPA / ITO working electrode and the V2O5 / ITO counter electrode to form a sandwich structure.

[0154] Step 3: Use photocuring adhesive to stick the copper tape to the positive and negative poles of the device to obtain the electrochromic capacitor window.

[0155] The preparation method of the EPA / ITO working electrode described in step 1 is as follows:

[0156] ① Dissolve 12 mg EPA in 1 mL DMF to prepare a uniform solution;

[0157] ②, drop the EPA DMF solution onto the ITO glass substrate and spin coat at 3000r / min for 30 seconds to form a uniform film;

[0158] ③. Transfer the above-mentioned ITO glass substrate with a uniform thin film to a vacuum oven at 45° C. and dry it for 24 hours to obtain an EPA / ITO working electrode.

[0159] Step 1 V 2 O 5 / ITO counter electrode preparation method is as follows:

[0160] ①, at 60℃, V 2 O 5 (1.2 g) and NaCl (1.44 g) were stirred in 100 mL of deionized water for 36 h until a color transition from yellow to brown occurred;

[0161] ② Centrifuge the mixture at 6000r / min three times, rinse with deionized water and ethanol until colorless, and collect the precipitate;

[0162] ③. The above precipitate was transferred to a vacuum oven at 45°C and dried for 24 hours to obtain V 2 O 5 Nanowires;

[0163] ④, 2 mg of V 2 O 5 The nanowires were uniformly dispersed in 5 mL of deionized water. 2 O 5 The nanowire solution was spin-coated at 2000 r / min for 30 s to form a uniform film;

[0164] ⑤, anneal at 60℃ for 1 hour to obtain V 2 O 5 / ITO counter electrode.

[0165] Figure 6 CV test of EPA / ITO working electrode prepared from electroactive polyamide EPA (where the electrolyte is 0.1M LiClO 4 / ACN solution, the scan rate was 10 mV s -1 To 100mV s -1 , the voltage window is -0.5 to 1.0 V). The curve shows three pairs of redox peaks, at 0.01 V / -0.19 V, 0.29 V / 0.17 V and 0.57 V / 0.42 V (vs. Ag / Ag +). This is because EPA has four redox structural states during the electrochemical process, namely, reduced state, semi-oxidized state I, semi-oxidized state II, and fully oxidized state. In addition, the peak shape of the CV curve also shows that the EPA / ITO working electrode has good energy storage performance.

[0166] Figure 7 The transmittance spectrum curve of the EPA / ITO working electrode prepared from the electroactive polyamide EPA at -0.5 to 1V voltage is shown. The EPA / ITO working electrode shows a large transmittance response in both the visible and near-infrared regions. The maximum transmittance contrast is 58.41% and 54.62% at 650 nm and 1200 nm, respectively. The transmittance of the EPA / ITO working electrode changes significantly after applying different voltages, which should be attributed to the change of the redox state of the pentaphenylamine segment during the electrochemical process.

[0167] Figure 8 V 2 O 5 The scanning electron microscope image of the / ITO counter electrode confirms that V 2 O 5 Nanowires were successfully prepared. 2 O 5 The nanowire morphology increases the specific surface area during the electrochemical process, which is beneficial to improving the electrical energy storage performance.

[0168] Fig. 9 The CV test of the assembled electrochromic capacitor window was performed at 10 mV s -1 To 100mV s -1 At a scan rate of , the voltage window of the capacitor window can reach 2V, and the redox peak current of the electrochromic capacitor window gradually increases with the increase of the scan rate, revealing its excellent electrochemical kinetics. It can also be seen from the shape of the CV curve that the capacitor window also has excellent energy storage performance.

[0169] Fig.10 The transmittance spectrum curve of the assembled electrochromic capacitor window between 300-2000nm is obtained by combining an electrochemical workstation with a UV-visible-near infrared spectrometer. The electrochromic capacitor window shows a large transmittance change in both the visible light and near-infrared regions, with the highest transmittances at 650nm and 1200nm being 56.57% and 53.29%, respectively. This shows that in the process of mutual conversion between 0V and 2V, the capacitor window can achieve dual-band modulation of visible light and solar radiation.

[0170] Fig.11The assembled electrochromic capacitor window was tested with a square wave at 650nm. Under alternating voltages of 0V and 2V, the maximum transmittance of the capacitor window reached 52.33%. The color conversion time is defined as the time required to achieve a maximum transmittance change of 90%. During the bleaching / coloring process, the capacitor window showed a relatively fast color conversion time of 4.26 seconds / 4.57 seconds, respectively. This fully demonstrates the excellent electrochromic properties of the electrochromic capacitor window.

[0171] Fig.12 The assembled electrochromic capacitor window was tested by a square wave at 1200nm. Under the alternating voltage of 0V and 2V, the maximum transmittance of the capacitor window reached 48.68%. The time required to reach the maximum transmittance change of 90% is also defined as the color conversion time. During the coloring / bleaching process, the color conversion time of the capacitor window was 4.31 seconds / 4.93 seconds respectively. This shows that the electrochromic capacitor window has excellent electrochromic properties in the near-infrared region similar to those in the visible light region.

[0172] Fig.13 Long-term cycle test of the assembled electrochromic capacitive window at 0.2 mA cm -2 The electrochemical durability of the electrochromic capacitor window was studied by long-cycle electrostatic charge and discharge tests at a current density of . After 10,000 long cycles, the coulombic efficiency of the capacitor window remained at 100% without significant changes. Compared with the first time, the capacity retention rate of the 10,000th time only decayed to 79%. The ideal results of these electrochemical durability tests all demonstrate the feasibility and reliability of the electrochromic capacitor window during long-term use.

[0173] Those skilled in the art can understand that the above-mentioned embodiments are specific examples for implementing the present application, and in practical applications, various changes can be made to them in form and detail without departing from the spirit and scope of the present application. Any person skilled in the art can make their own changes and modifications without departing from the spirit and scope of the present application, so the scope of protection of the present application shall be based on the scope defined in the claims.

Claims

1. Application of an electroactive polyamide EPA containing pentaphenylamine in the main chain in an electrochromic capacitor window, characterized in that: The polyamide has a repeating unit having a structure shown in formula (I): ; Capacitor window assembly includes the following steps: C. Preparation of EPA / ITO working electrode, V2O5 / ITO counter electrode and gel electrolyte; D. Place the gel electrolyte between the EPA / ITO working electrode and the V2O5 / ITO counter electrode to form a sandwich structure; E. Use photocuring adhesive to stick the copper tape to the positive and negative poles of the device to obtain an electrochromic capacitor window.

2. The use of an electroactive polyamide EPA containing pentaphenylamine in the main chain in an electrochromic capacitor window according to claim 1, characterized in that: The electroactive polyamide EPA containing pentaphenylamine in the main chain was prepared according to the following steps: A. Synthesis of electroactive amide monomer EA: A1. Place 14-28 mmol of p-aminodiphenylamine and 30 mL of dry DMF solution in a reaction vessel, and perform ultrasonic treatment for 15 minutes; A2, dissolve 5-10 mmol of terephthaloyl chloride in 20 mL of DMF; A3, dropwise adding the DMF solution of terephthaloyl chloride into the DMF solution of p-aminodiphenylamine, and reacting for 6 hours; A4. Pour the mixed solution into 300 mL of ice water for precipitation, and wash the resulting precipitate with distilled water, ethanol, dichloromethane and ether in sequence; A5, dried under vacuum at 45°C for 24 hours to obtain gray-green solid EA; B. Synthesis of electroactive polyamide EPA: B1. Add 2-4 mmol of EA and 2.1-4.2 mmol of p-phenylenediamine into a reaction vessel, and pour in 40 mL of DMF solution; B2. During the stirring process, 15 mL of 3 mol / L hydrochloric acid solution was added dropwise to the above DMF solution to form a uniform dispersion; B3. Transfer 4-8 mmol of ammonium persulfate into 10 mL of 3 mol / L hydrochloric acid; B4, adding the hydrochloric acid solution of ammonium persulfate dropwise to the above dispersion for 30 minutes, and reacting at room temperature for 24 hours; B5. Pour the reaction mixture into 300 mL of ice water for precipitation, filter the precipitate, and wash with distilled water, ethanol and acetone in sequence until it is colorless; B6. Disperse the precipitate with 2.5 mol / L ammonia solution, reduce it with hydrazine hydrate, transfer it to a 45°C vacuum oven, and dry it for 24 hours to obtain dark green solid EPA.

3. The use of an electroactive polyamide EPA containing pentaphenylamine in the main chain in an electrochromic capacitor window according to claim 2, characterized in that: In step A, the molar ratio of p-aminodiphenylamine to terephthaloyl chloride is 2.8:

1.

4. The use of an electroactive polyamide EPA containing pentaphenylamine in the main chain in an electrochromic capacitor window according to claim 2, characterized in that: In step B6, the molar ratio of the amide monomer EA to the hydrazine hydrate is 1:

6.

5. The use of an electroactive polyamide EPA containing pentaphenylamine in the main chain in an electrochromic capacitor window according to claim 1, characterized in that: In step C, the EPA / ITO working electrode preparation method is as follows: C1. Dissolve 10-12 mg EPA in 1 mL DMF to prepare a uniform solution. C2, drop the EPA DMF solution onto the ITO glass substrate and spin coat at 3000 r / min for 30 seconds to form a uniform film; C3. The ITO glass substrate with the uniform thin film was transferred to a vacuum oven at 45° C. and dried for 24 hours to obtain an EPA / ITO working electrode.

6. The use of an electroactive polyamide EPA containing pentaphenylamine in the main chain in an electrochromic capacitor window according to claim 1, characterized in that: The method for preparing the V2O5 / ITO counter electrode in step C is as follows: C4. 1.0-1.2 g of V2O5 and 1.2-1.44 g of NaCl were stirred in 100 mL of deionized water at 60 °C for 36 hours until a color change from yellow to brown occurred; C5. Centrifuge the mixture at 6000 r / min for three times, rinse with deionized water and ethanol until colorless, and collect the precipitate; C6, transferring the above precipitate to a vacuum oven at 45°C and drying for 24 hours to obtain V2O5 nanowires; C7, 2 mg of V2O5 nanowires were uniformly dispersed in 5 mL of deionized water; then, the dispersed V2O5 nanowire solution was spin-coated at a speed of 2000 r / min for 30 seconds to form a uniform film; C8. Anneal at 60°C for 1 hour to obtain a V2O5 / ITO counter electrode.

7. The use of an electroactive polyamide EPA containing pentaphenylamine in the main chain in an electrochromic capacitor window according to claim 6, characterized in that: In step C4, the mass ratio of V2O5 to NaCl during the preparation of the V2O5 / ITO counter electrode is 1:1.2.

Citation Information

Patent Citations

  • All solid-state electrochromic intelligent glass and self-driving energy system thereof

    CN106371259A