Ultra-high strength spring steel and preparation method thereof
By adopting the chemical composition and optimization process of manganese-aluminum-nitrogen microalloyation in spring steel, the problems of insufficient strength and high production costs of existing spring steel are solved, and high-strength and low-cost ultra-high-strength spring steel are realized , suitable for high-end equipment manufacturing industry.
Patent Information
- Application Number
- CN202310583654.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-05-23
AI Technical Summary
The existing spring steel is insufficient to meet the needs of high-performance, high-speed engines, aerospace and other fields, and the production costs are high, resulting in a small share of domestic spring products in the high-end market, unstable performance and unstable service life.
Ultra-high strength spring steel containing manganese-aluminum-nitrogen microalloy is used, with chemical compositions of C: 0.45-0.60%, Si: 0.15-0.35%, Mn: 6.0-12.0%, Al: 1.0-3.0%, Cr: 0.30-0.50%, Mo: 0.10-0.25%, V: 0.10-0.50%, Nb: 0.025-0.04%, N: 0.005-0.015%, improve the mechanical strength of spring steel by solid solution strengthening and refining grain structure , elongation and fatigue resistance, and reduce production costs through optimized processes.
It has achieved high mechanical strength, high elongation and good fatigue resistance of ultra-high strength spring steel, low cost, suitable for industrial production, and suitable for high-demand industries, such as equipment manufacturing.
Smart Images

Figure CN116657039B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of special steel production, and specifically relates to an ultra-high strength (2GPa) spring steel and a preparation method thereof. Background Art
[0002] Springs, bolts and gears constitute the three basic parts of machinery. There are many varieties of springs, which are widely used in the automotive industry, mechanical equipment, light industry, electric power industry, aerospace, rail transportation and other industries. The role of springs is extremely important. They play various complex working conditions such as buffering, shock absorption, energy storage, connection, support, and force transmission in various mechanical equipment. Their good comprehensive service performance is the basis for the safe operation of mechanical equipment. Improving the quality level of springs is a prerequisite for ensuring the performance improvement of the main machine of mechanical equipment. Springs work under alternating stresses such as periodic bending and torsion, and are subjected to various effects such as tension, compression, torsion, impact, fatigue and corrosion. Sometimes they have to work in very harsh and complex working environments, such as high temperature, low temperature, corrosion, static load, etc. In recent years, with the rapid development of industries such as automobiles and rail transportation, in order to save energy and resources, the lightweight design of automobiles and rail transportation has become more and more urgent for spring weight reduction, and the demand for ultra-high strength springs has increased. However, the current strength of domestic spring steel is only about 1350MPa, which seriously restricts the development of new energy vehicles and the weight reduction and emission reduction of various types of vehicles, and cannot meet the development needs of high-performance and high-speed engines, especially in the fields of aviation and aerospace. The development of high-performance spring steel with ultra-high strength, high elongation, high cross-sectional shrinkage and fatigue resistance will be an inevitable trend to improve my country's independent supporting capabilities for high-end equipment parts and effectively replace imports.
[0003] In the field of global high-performance spring steel research and development and production, industry giants such as Kobe Steel of Japan lead the development of global spring steel. my country's spring products are large in scale and diverse in categories, but the market share of high-end spring products is small, that is, the industrial structure of my country's spring industry has long formed a passive situation in which low-end ordinary springs are in oversupply and high-end products (high strength, high stress, special parts, special materials) are in short supply. Spring products can no longer fully meet the development needs of the high-end equipment manufacturing industry. Suspension springs, valve springs, clutch springs for cars, and high-grade springs for locomotives, machinery, electricity, military and other industries still need to be imported. In addition, the performance of my country's spring products is still somewhat different from similar foreign products, such as the load accuracy and verticality accuracy of the springs. The performance is mainly reflected in the unstable performance, the large discreteness of some important quality indicators, and the unstable service life. Especially when the host requires the spring to work under high-speed and high-stress conditions, the contradiction is more prominent.
[0004] Spring steel is divided into non-alloy spring steel (carbon spring steel) and alloy spring steel according to chemical composition. At present, the springs used in various countries are mainly high-quality carbon steel with a carbon content of 0.3-0.9wt.% and alloy spring steel containing Cr-Si, Cr-Mn, Si-Mn, Cr-V and other alloy composition systems. Carbon spring steel is mainly used to make springs such as scroll springs and leaf springs, while most other springs such as suspension springs and valve springs are made of alloy spring steel. Si-Mn spring steel has good anti-elasticity and low production cost, and has become the main spring steel production system in my country. However, Si-Mn spring steel also has certain problems. The surface of the spring steel is easy to decarburize during heat treatment, and the problem of insufficient hardenability limits its development. In foreign countries, most countries use Cr-Mn and Cr-V alloy steels to prepare spring steel. The reason is that these two alloy spring steels have good hardenability during heat treatment and the surface of the spring steel is not easy to decarburize. Based on the above system, various countries are further developing spring steel with better performance. The main idea is to add alloy elements such as Mo, W, and V. The main purpose is to improve the hardenability of spring steel, refine the grains, and reduce the grain size, so as to achieve the purpose of improving the organization and performance of spring steel.
[0005] In recent years, with the high-quality development of the dual-carbon economy and equipment manufacturing industry, spring products not only need to achieve higher mechanical properties and better fatigue performance, but also need to have lower production costs. Therefore, the main development directions of spring steel are: first, continue to develop the existing spring steel system, adopt different processes or add trace elements to further develop its potential; second, develop a new spring steel system. The development of a new spring steel system requires a lot of time and cost, so relatively few countries and regions have developed it. The SAE9254 and 54SiCrV6 grades of springs that are widely used in the market now have too low strength, and the production cost of 54SiCrV6 is high; the UHS2000 grade spring has a higher strength, but its cost is extremely high. Aiming at the pain points and difficulties in the industry, the present invention invents an ultra-high strength spring steel containing manganese-aluminum-nitrogen microalloying, which has the advantages of high mechanical strength, large elongation, high cross-sectional shrinkage, and good fatigue resistance; at the same time, the preparation method of this ultra-high strength spring steel is simple and easy, the production cost is low, and it is suitable for industrial production. Summary of the invention
[0006] In view of the current problem of lack of high-strength spring steel products, the present invention provides an ultra-high-strength spring steel having the advantages of high mechanical strength, large elongation, high cross-sectional shrinkage and good fatigue resistance.
[0007] Another object of the present invention is to provide a method for preparing the ultra-high strength spring steel, which is simple and suitable for industrial production.
[0008] To achieve the above purpose, the present invention adopts the following technical solution.
[0009] An ultra-high strength spring steel, belonging to a manganese-aluminum-nitrogen microalloyed spring steel, comprising the following chemical components in mass percentage:
[0010] The main chemical components are: C: 0.45-0.60%, Si: 0.15-0.35%, Mn: 6.0-12.0%, Al: 1.0-3.0%, Cr: 0.30-0.50%, Mo: 0.10-0.25%, V: 0.10-0.50%, Nb: 0.025-0.04%, N: 0.005-0.015%;
[0011] The chemical composition of impurities is: Pb≤0.03%, Sn≤0.03%, Zn≤0.03%, Sb≤0.03%, Bi≤0.03%, O2≤15ppm, H2≤15ppm; S≤0.02%, P≤0.02%, Cu≤0.2%, Ni≤0.35%;
[0012] The balance is iron and unavoidable impurities.
[0013] In the present invention, the addition amount and function of each chemical component are as follows:
[0014] Carbon (C) improves the elastic strength, hardness and wear resistance of spring steel through solid solution strengthening, but reduces the plasticity, toughness and fatigue strength of spring steel. When C is controlled within 0.45-0.60wt.%, it can obtain the best combination of strength, fatigue life and economic benefits when it is present with other alloying elements. The C content used in the present invention is less than that of conventional spring steel. When the content is within this range, the martensitic structure morphology can be changed and the toughness of spring steel can be improved.
[0015] Silicon (Si) strengthens ferrite by solid solution and improves the elasticity of steel, but weakens the plasticity and toughness of steel, and sharply increases the tendency of decarburization and graphitization, produces inclusions, and deteriorates the fatigue performance of springs. Therefore, in the present invention, it is found that when the silicon content is controlled within 0.15-0.35wt.%, the effect on fatigue strength is the lowest. The Si content used in the present invention is less than that of conventional spring steel, which can reduce the rejection of carbon and reduce decarburization.
[0016] Manganese (Mn) can improve the strength of steel through solid solution, improve the hardenability of steel, reduce carbon rejection, and reduce decarburization. The Mn content used in the present invention is much higher than that of conventional spring steel. The purpose is to utilize its interaction with aluminum and nitrogen to improve the dislocation migration ability, thereby greatly improving the strength without reducing the toughness of the steel. However, excessive Mn will promote temper brittleness, so the Mn content needs to be controlled at 6.0-12.0wt.%.
[0017] Aluminum (Al) can refine the grain structure of steel, inhibit the aging of low-carbon steel, reduce the sensitivity of notches, especially reduce the toughness-brittleness transition temperature of steel, and improve the toughness of steel at low temperatures. This invention introduces Al into spring steel for the first time, with the purpose of using the affinity of Al and nitrogen to play the role of deoxidation, nitrogen determination and grain refinement, and can also greatly improve the strength, low-temperature toughness and fatigue strength. However, excessive aluminum affects the hot working properties of steel. Through experiments, the optimal Al content needs to be controlled at 1.0-3.0wt.%.
[0018] Chromium (Cr) improves the strength of steel by solid solution, and can also improve the hardenability of steel and the tempering stability, which is beneficial to improving the performance and dispersion precipitation of spring steel. However, the Cr content used in the present invention is much smaller than that of conventional spring steel, in order to prevent excessive chromium from easily forming chromium carbide and reducing the plasticity and toughness of steel. Therefore, the Cr content is controlled at 0.30-0.50wt.%.
[0019] Molybdenum (Mo) improves the strength of steel through solid solution, strongly improves the hardenability of steel, stabilizes carbon elements, and is beneficial to improving the strength of spring steel. However, excessive Mo will change the quenching curve of steel, tending to form feathery bainite, which is not conducive to the fatigue strength of spring steel. Therefore, the Mo content needs to be controlled to 0.10-0.25wt.%.
[0020] Vanadium (V) and niobium (Nb) form dispersed and fine vanadium carbide (VC), niobium carbide (NbC), vanadium nitride (VN) or niobium nitride (NbN) in steel, which drastically strengthen the matrix and refine the grain boundaries to prevent the growth of grains. Therefore, a fine and high-strength structure can be obtained, which greatly improves the strength and fatigue performance of spring steel. However, when a single element is excessive, the particles are easily coarsened and lose their excellent effects. Therefore, the present invention adopts the comprehensive functions of the two elements. After optimization, the optimal content is V: 0.10-0.50wt.%; Nb: 0.025-0.04wt.%.
[0021] Cr, Mo, V and Nb are precious elements and are used in very small amounts in the present invention to reduce production costs.
[0022] The role of nitrogen (N) in steel is similar to that of carbon. It can improve the elasticity, strength and hardness of steel through stronger solid solution strengthening, but the weakening of the plasticity, toughness and fatigue strength of spring steel is smaller than that of carbon. In particular, the formed martensite is a Fe-CN structure with higher fatigue strength. Nitrogen-added microalloyed spring steel can have higher strength, toughness and fatigue life. 50-150ppm N content is the optimal N content determined by the present invention.
[0023] Sulfur (S) or phosphorus (P) forms inclusions with alloying elements, such as MnS, which not only offsets the beneficial effects of alloying elements, but also causes S and P to segregate, weaken the toughness of the steel, and become a source of fatigue cracks, seriously reducing the fatigue strength of the spring. Therefore, the S and P content in spring steel should be strictly controlled within 0.02wt.%.
[0024] Copper (Cu) will seriously reduce the thermoplasticity of the material. Since the spring has to undergo subsequent hot processing, a high Cu content is prone to microcracks, which seriously affects the strength of the spring. Therefore, the Cu content should be strictly controlled to ≤0.2wt.%.
[0025] Nickel (Ni) can improve the strength and toughness of steel, reduce the brittle transition temperature, and especially improve hardenability, but the price of nickel is extremely high, so other alloys are used as much as possible to meet the performance requirements. Within the content range of other elements, the present invention does not need to add Ni to meet the strength and toughness requirements. Ni≤0.35wt.% in the raw material is mainly the inevitable introduction in the raw material.
[0026] The method for preparing the ultra-high strength spring steel comprises the following steps:
[0027] The spring steel raw materials are sequentially smelted, refined, RH vacuum degassed, continuously cast into steel ingots, the steel ingots are peeled, continuously hot rolled, and controlled cooled to obtain ultra-high strength spring steel.
[0028] In order to reduce costs, the above-mentioned spring steel raw materials can use some scrap steel, but scrap steel contains impurities such as copper. Therefore, the amount of scrap steel needs to be controlled within 20% of the total mass of the spring steel raw materials.
[0029] Specifically, the preparation process of ultra-high strength spring steel includes: putting raw materials into the converter, controlling the mass percentage of scrap steel in the raw materials. In order to control the impurity content, electromagnetic stirring and RH vacuum degassing are used in the whole process of secondary refining, which can make the fiber structure uniform, with fewer bubbles, fewer pores, and dense organization. After the vacuum degassing is completed, continuous casting is carried out to form a stable macroscopic organization, and continuous heating and rolling can ensure uniform size organization; controlling the cooling temperature can reduce the decarburization layer and ensure the shear hardness. After cooling to room temperature, steel is obtained.
[0030] Furthermore, the optimized process parameters in the above process are as follows:
[0031] The melting temperature is 1630°C-1700°C, and the time is 25-60 minutes. The refining temperature is 1500°C-1550°C, and the time is 20-60 minutes. In order to make the microstructure uniform and prevent the segregation of alloy elements, electromagnetic stirring is used in the refining process.
[0032] The parameters of RH vacuum degassing are: vacuum degree ≤ 130Pa, time 20-60 minutes.
[0033] The rolling reduction ratio of the ingot size obtained by continuous casting to the spring steel size is greater than 15:1. The cooling process of continuous casting needs to be cooled to below 1150℃ at 25℃-35℃ / min, and then naturally cooled to room temperature. This can limit the inclusions to the center line of the ingot as much as possible, and reduce the damage to the performance of the product after the steel is rolled.
[0034] The depth of ingot peeling is not less than 3.0mm.
[0035] The starting rolling temperature of continuous hot rolling is 900℃-1000℃, and the final rolling temperature is 780℃-900℃. Continuous hot rolling needs to be carried out in the austenite region to give full play to the best deformation properties of the material and provide favorable conditions for subsequent cooling.
[0036] The specific steps of controlled cooling are: fast cooling to 600℃ at a speed of not less than 30℃ / min, and then slowly cooling to room temperature at a speed of not more than 10℃ / min. This can prevent surface decarburization and maintain a low hardness to facilitate subsequent shearing processing.
[0037] The ultra-high strength spring steel obtained by the above preparation method has a hardness of ≤HB350, a semi-decarburized layer of ≤0.20 mm, and no full decarburized layer.
[0038] In order to further improve the performance of spring steel, heat treatment is required after processing and forming to obtain the finished product. The specific heat treatment process is "quenching + tempering" heat treatment. During the heat treatment process, the quenching method is oil quenching, the quenching temperature is 840-890℃, and the holding time is 1.0-1.3min / mm; the tempering temperature is 380℃-500℃. After the above heat treatment, metallographic detection found that the microstructure of the spring steel is >95% troostite and a small amount of ferrite, and only troostite and ferrite, without other tissues.
[0039] After heat treatment, the finished product has a tensile strength of more than 2000MPa, a yield strength of more than 1850MPa, an elongation of ≥7%, a cross-sectional shrinkage of ≥25%, fatigue cycles of more than 350,000 cycles, and a grain size greater than ASTM grade 9.0.
[0040] The ultra-high strength spring steel obtained by the above preparation method has an application thickness of 6-50 mm or an application diameter of 6-35 mm.
[0041] The present invention has the following advantages:
[0042] The spring steel provided by the invention has high mechanical strength, large elongation, high cross-sectional shrinkage, and good fatigue resistance, and can be used in high-requirement industries such as equipment manufacturing; the cost is lower than the current market spring steel. The preparation method provided by the invention is scientific, reasonable, simple and easy to implement, and suitable for mass industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 This is the metallographic diagram of spring steel without heat treatment;
[0044] Figure 2 is the metallographic diagram of Example 1;
[0045] Figure 3 is the metallographic diagram of Example 2;
[0046] Figure 4 This is the metallographic diagram of Example 3. DETAILED DESCRIPTION
[0047] The present invention is further described below in conjunction with the examples and drawings, but the present invention is not limited by the following examples. All raw materials used in the examples are commercially available unless otherwise specified.
[0048] Example 1 Preparation of ultra-high strength spring steel
[0049] The chemical composition weight percentage of the steel in this embodiment is shown in Table 1.
[0050] The following steps are used to produce ultra-high strength spring steel:
[0051] The molten iron was added into a 25-ton induction heating furnace and smelted at 1680°C. After 45 minutes, the steel was tapped and 18.0wt.% scrap steel was added to adjust the temperature to 1600°C and transferred to a refining furnace. Under electromagnetic stirring, alloy materials such as ferrosilicon, ferromanganese, ferrochrome-molybdenum, ferrovanadium, ferroniobium and manganese nitride were added respectively. Pure aluminum wire was fed at 1535±15°C and the chemical composition was adjusted for 40 minutes before RH vacuum degassing (vacuum degree ≤ 130Pa) was performed. ); then continuously cast into 200×200mm ingot, cooled to 1150℃ at a speed of 28℃ / min, and then air-cooled to room temperature; then the ingot was peeled, peeled to a depth of 3.2mm, and then heated to 1150℃, and finally continuously rolled into 24×89mm spring strip steel, with a starting rolling temperature of 1050℃ and a final rolling temperature of 860℃. After rolling, it was quickly cooled to 600℃ at a speed of 37℃ / min, and then slowly cooled to room temperature at a speed of 8℃ / min. According to the above method, a 24×89mm strip steel was obtained, and its chemical composition was shown in Table 1 after inspection. Its metallographic diagram is shown in Figure 1 As shown in the figure, the microstructure of the spring steel without heat treatment is mainly pearlite and ferrite.
[0052] The strip steel obtained in Example 1 was further processed into a single leaf spring, and after being kept at 880°C for 20 minutes, oil quenched and tempered at 460°C for 45 minutes, a leaf spring product was obtained. Samples were taken from the leaf spring product obtained in Example 1, and then metallographic specimens were prepared. The metallographic structure is as follows: Figure 2 As shown. Figure 2 It can be seen that the microstructure of the spring steel prepared in Example 1 contains uniform troostite and a small amount of ferrite, and the troostite exceeds >95%. Figure 1 Compared with the above, the microstructure of the spring steel obtained in Example 1 is significantly improved. Furthermore, the prepared leaf spring product is subjected to tensile specimen processing and tensile test according to GB / T228-2002, and the yield strength, elongation and cross-sectional shrinkage are tested. The assembled leaf spring is subjected to fatigue test according to GB / T228-2002, and the test results are shown in Table 2, and the tensile strength reaches 2193 MPa.
[0053] Example 2 Preparation of ultra-high strength spring steel
[0054] The chemical composition weight percentage of the steel in this embodiment is shown in Table 1.
[0055] The following steps are used to produce ultra-high strength spring steel:
[0056] The molten iron was added into a 60-ton converter and smelted at 1630°C. After 60 minutes, the steel was tapped and 15.0% scrap steel was added to adjust the temperature to 1650°C and transferred to a refining furnace. Under electromagnetic stirring, alloy materials such as ferrosilicon, ferromanganese, ferrochrome-molybdenum, ferrovanadium, ferroniobium and manganese nitride were added respectively. After adjusting the chemical composition at 1515±15°C for 60 minutes, vacuum degassing was performed (under the condition of vacuum degree ≤130Pa). Subsequently, the 200×200mm ingot was continuously cast, cooled to 1150°C at a speed of 30°C / min, and then air-cooled to room temperature. The ingot was then peeled, and after peeling off 3.5mm in depth, it was heated to 1200°C and finally continuously rolled into 24×89mm spring strip steel, with a starting rolling temperature of 950°C and a final rolling temperature of 850°C. After rolling, it was rapidly cooled to 600°C at a speed of 35°C / min, and then the temperature was slowly cooled to room temperature at a speed of 10°C / min. According to the above method, a 24×89 mm strip steel was obtained, and its chemical composition was shown in Table 1.
[0057] The strip steel obtained in Example 2 was further processed into a single leaf spring, and after being kept at 850°C for 20 minutes, oil quenched and tempered at 480°C for 45 minutes, a leaf spring product was obtained. Samples were taken from the leaf spring product obtained in Example 2, and then metallographic specimens were prepared. The metallographic structure is as follows: Figure 3 As shown. Figure 3 It can be seen that the microstructure of the spring steel prepared in Example 2 contains uniform troostite and a small amount of ferrite, and the troostite exceeds >95%. Figure 1 In comparison, the microstructure of the spring steel obtained in Example 2 is significantly improved. Furthermore, the leaf spring product is subjected to tensile specimen processing and tensile test according to GB / T228-2002, and the yield strength, elongation and cross-sectional reduction are tested. The assembled leaf spring is subjected to fatigue test according to GB / T228-2002, and the test results are shown in Table 2, and the tensile strength reaches 2183 MPa.
[0058] Example 3 Preparation of ultra-high strength spring steel
[0059] The chemical composition weight percentage of the steel in this embodiment is shown in Table 1.
[0060] The following steps are used to produce ultra-high strength spring steel:
[0061] The molten iron was added into a 120-ton converter and smelted at 1700°C. After 25 minutes, the steel was tapped and 16% scrap steel was added to adjust the temperature to 1650°C and then transferred to a refining furnace. Under electromagnetic stirring, alloy materials such as ferrosilicon, ferromanganese, ferrochromium-molybdenum, ferrovanadium, ferroniobium and manganese nitride were added respectively. After adjusting the chemical composition at 1535±15°C for 30 minutes, vacuum degassing was performed (under the condition of vacuum degree ≤130Pa). Subsequently, the 200×200mm ingot was continuously cast, cooled to 1150°C at a speed of 35°C / min, and then air-cooled to room temperature. The ingot was then peeled, and after peeling 3.0mm in depth, it was heated to 1200°C and finally continuously rolled into 24×89mm spring strip steel. The starting rolling temperature was 900°C, the final rolling temperature was 900°C, and after rolling, it was rapidly cooled to 600°C at a speed of 40°C / min, and then the temperature was slowly cooled to room temperature at a speed of 9°C / min. According to the above method, a 24×89 mm strip steel was obtained, and its chemical composition was shown in Table 1.
[0062] The strip steel obtained in Example 3 was further processed into a single leaf spring, and after being kept at 900°C for 20 minutes, oil quenched and tempered at 500°C for 45 minutes, a leaf spring product was obtained. Samples were taken from the leaf spring product obtained in Example 3, and then metallographic specimens were prepared. The metallographic structure of the leaf spring product was as follows: Figure 4 As shown. Figure 4 It can be seen that the microstructure of the spring steel prepared in Example 3 contains uniform troostite and a small amount of ferrite, and the troostite accounts for more than 95%. Figure 1 In comparison, the microstructure of the spring steel obtained in Example 3 is significantly improved. Furthermore, the leaf spring product is subjected to tensile specimen processing and tensile test according to GB / T228-2002, and the yield strength, elongation and cross-sectional reduction are tested. The assembled leaf spring is subjected to fatigue test according to GB / T228-2002, and the test results are shown in Table 2, and the tensile strength reaches 2156 MPa.
[0063] Comparative Example
[0064] The chemical compositions of three commonly used spring steels, namely standard steel SAE9260, standard steel SAE5160 and standard steel SAE6150, are shown in Table 1. Then the three standard steels are processed into single leaf springs according to the process of Application Example 3, that is, after being kept at 900°C for 20 minutes, oil quenched and tempered at 500°C for 45 minutes, leaf spring products are obtained. The leaf spring products are processed and tested for tensile specimens according to GB / T228-2002, and the yield strength, elongation and section reduction are tested. The assembled leaf springs are subjected to fatigue tests according to GB / T228-2002, and the test results are shown in Table 2.
[0065] Table 1 Comparison of chemical composition of different steels (wt.%)
[0066]
[0067] Table 2 Performance test results of different finished products
[0068]
[0069] It can be seen from the results in Table 2 that, while maintaining the same level of plasticity, toughness, cross-sectional shrinkage Z, elongation A, etc., the strength of the leaf spring products of the spring steel prepared in Examples 1 to 3 is greatly improved; compared with the standard steel 9260, the yield strength (Rp 0.2 ) is increased by up to about 1.05 times, the tensile strength (Rm) is increased by up to about 1.02 times, and the fatigue strength is increased by more than 4 times. Therefore, the ultra-high strength spring steel of the present invention is particularly suitable for the manufacture and production of weight-reducing leaf springs.
Claims
1. A 2GPa ultra-high strength spring steel, It is characterized in that The chemical composition by mass ratio is as follows: The main chemical components are: C: 0.45-0.60%, Si: 0.15-0.35%, Mn: 6.0-12.0%, Al: 1.0-3.0%, Cr: 0.30-0.50%, Mo: 0.10-0.25%, V: 0.10-0.50%, Nb: 0.025-0.04%, N: 0.005-0.015%; Controlled impurity chemical composition: Pb≤0.03%, Sn≤0.03%, Zn≤0.03%, Sb≤0.03%, Bi≤0.03%, O 2 ≤15ppm, H 2 ≤15ppm; S≤0.02%, P≤0.02%, Cu≤0.2%, Ni≤0.35%; The balance is iron and unavoidable impurities.
2. A method for preparing the 2GPa ultra-high strength spring steel as claimed in claim 1, It is characterized in that The following steps are involved: The spring steel raw materials are sequentially melted, refined, RH vacuum degassed, continuously cast into steel ingots, the steel ingots are peeled, continuously hot rolled, and controlled cooled to obtain ultra-high strength spring steel.
3. The preparation method according to claim 2, It is characterized in that The smelting temperature is 1630-1700°C, and the time is 25-60 minutes; the refining temperature is 1500-1550°C, and the time is 20-60 minutes; The vacuum degree of RH vacuum degassing is ≤130Pa; the vacuum time is 20-60 minutes.
4. The preparation method according to claim 2, It is characterized in that Electromagnetic stirring is used in the refining process.
5. The preparation method according to claim 2, It is characterized in that The cooling process of continuous casting is to first cool down to below 1150℃ at 25℃-35℃ / min, and then cool naturally to room temperature; The specific steps of controlled cooling are: rapidly cooling to 600°C at a speed of not less than 30°C / min, and then slowly cooling to room temperature at a speed of not more than 10°C / min; The starting temperature of hot rolling is 900-1000℃, and the final rolling temperature is 780-900℃.
6. The preparation method according to claim 2, It is characterized in that The peeling depth of the steel ingot is at least 3.0 mm; and the compression ratio of continuous hot rolling is greater than 15:
1.
7. The preparation method according to any one of claims 2 to 6, It is characterized in that The hardness of the obtained spring steel is ≤HB350, the semi-decarburized layer is less than or equal to 0.20 mm, and there is no full decarburized layer.
8. The preparation method according to claim 2, It is characterized in that It also includes heat treatment; the heat treatment method is quenching + tempering; the quenching method is oil quenching, the quenching temperature is 840-890℃, and the holding time is 1.0-1.3min / mm; the tempering temperature is 380℃-500℃.
9. The preparation method according to claim 8, It is characterized in that The microstructure of the obtained spring steel is >95% troostite and a small amount of ferrite, and only troostite and ferrite, without other tissues; The obtained spring steel has a tensile strength of ≥2000MPa, a yield strength of ≥1850MPa, an elongation of ≥7%, a cross-sectional shrinkage of ≥25%, a fatigue cycle of more than 350000; and a grain size greater than ASTM grade 9.
0.
10. The preparation method according to claim 8, It is characterized in that The obtained spring steel has an application thickness of 6-50 mm and an application diameter of 6-35 mm.