A silicon carbide wafer with uniformly distributed stress and a method for non-destructively and accurately measuring the stress of the wafer in all directions

Through XRD diffraction testing and rotation technology, the cost and damage problems of silicon carbide wafer stress detection are solved, and lossless and accurate allotropic stress detection is achieved, ensuring the uniform mechanical performance of the wafer and the stability of the device.

CN116657249BActive Publication Date: 2024-11-12SICC SHANGHAI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310637184.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-11-12
Estimated Expiration
2043-05-31

AI Technical Summary

Technical Problem

The existing silicon carbide wafer stress detection methods have problems such as expensive equipment, poor accuracy, or inability to achieve non-destructive testing, especially the inability to accurately measure anisotropic stress and industrial applications.

Method used

Through XRD diffraction testing, the in-plane and inter-plane rotation are combined, the anisotropic strain value is calculated and the anisotropic stress is calculated using the elastic constant. It provides a lossless and accurate method to detect the anisotropic stress of the silicon carbide wafer to ensure that the stress is uniformly distributed .

Benefits of technology

It realizes lossless and accurate detection of the silicon carbide wafers, improves detection accuracy and reliability, and is suitable for industrial large-scale inspections, ensuring the uniformity of the mechanical properties of the wafer and the stability of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116657249B_ABST
    Figure CN116657249B_ABST
Patent Text Reader

Abstract

The present application discloses a silicon carbide wafer with uniformly distributed stress and a method for non-destructively and accurately measuring the isotropic stress of the wafer, belonging to the technical field of silicon carbide wafers and stress detection thereof. The determination method comprises the following steps: (1) performing an XRD diffraction test on the wafer, rotating the wafer in-plane and between-planes during the test, obtaining test results under at least 6 diffraction crystal planes, comparing the diffraction peaks of different diffraction crystal planes with the standard peaks of the corresponding diffraction crystal planes in the stress-free wafer, and obtaining the isotropic strain value of the wafer; (2) calculating the isotropic stress of the wafer based on the isotropic strain value and the elastic constant. The method can realize non-destructive and accurate detection of the isotropic stress of the wafer, provides a new idea for the analysis of the isotropic stress of the wafer, and can be extended to the standardized detection of the isotropic stress of the wafer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a silicon carbide wafer with uniformly distributed stress and a method for non-destructively and accurately measuring the stress of the wafer in all directions, belonging to the technical field of silicon carbide wafers and stress detection thereof. Background Art

[0002] There are several methods for detecting residual stress in silicon carbide, including neutron scattering, micro-Raman spectroscopy, optical interferometry, XRD diffraction, etc. Neutron scattering method requires a small-angle neutron diffractometer to analyze wafer stress. Currently, there are still few such diffractometers in the industry, mainly because the equipment is relatively expensive and cannot be industrialized for detection; Raman spectroscopy can test stress conditions at different depths according to different wavelengths, but it is currently impossible to directly use Raman spectroscopy to test anisotropic stress conditions in the surface; the test accuracy of optical interferometry is relatively poor, and it cannot distinguish anisotropic stress in the surface.

[0003] XRD diffraction method can obtain absolute stress parameters and is also a relatively convenient testing method. However, it is difficult and inaccurate to characterize the stress tensor of a single crystal using the traditional XRD diffraction method. Currently, anisotropic stress analysis can only be performed by cutting the wafer into small pieces. However, this detection method is a destructive detection method and cannot achieve non-destructive testing of the wafer. Summary of the invention

[0004] In order to solve the above problems, a silicon carbide wafer with isotropically distributed stress and a method for non-destructively and accurately measuring the isotropic stress of the wafer are provided. The isotropic stress values ​​of the silicon carbide wafer can be calculated through XRD diffraction testing. The first normal stress, the second normal stress and the third normal stress of the silicon carbide wafer are low and substantially the same. Therefore, a silicon carbide wafer with isotropically distributed stress is obtained, which can improve the quality of the wafer and its subsequent use value.

[0005] The method for determining the isotropic stress of a wafer rotates the wafer within and between planes during the test, calculates the isotropic strain values ​​of the wafer according to the diffraction peaks of different diffraction crystal planes, and calculates the isotropic stress of the wafer according to the isotropic strain values ​​and elastic constants. This method can achieve non-destructive and accurate detection of the isotropic stress of the wafer, provides a new idea for the analysis of the isotropic stress of the wafer, and can be promoted for standardized detection of the isotropic stress of the wafer.

[0006] According to one aspect of the present application, a silicon carbide wafer with isotropically distributed stress is provided, wherein the isotropic stress of the silicon carbide wafer is obtained by XRD diffraction testing, and the first normal stress, the second normal stress and the third normal stress of the silicon carbide wafer are all no greater than 60 MPa.

[0007] Optionally, the first shear stress, the second shear stress and the third shear stress of the silicon carbide wafer are all no greater than 30 MPa.

[0008] The first normal stress, the second normal stress and the third normal stress of the silicon carbide wafer are all no greater than 60 MPa, and the first shear stress, the second shear stress and the third shear stress are all no greater than 30 MPa.

[0009] The first positive stress is the stress along the X-axis direction, the second positive stress is the stress along the Y-axis direction, and the third positive stress is the stress along the Z-axis direction. The above-mentioned first positive stress, second positive stress and third positive stress represent the mechanical properties of the silicon carbide wafer. If the value is too large, it will cause damage to the wafer, microcracks or cracks. Therefore, the first positive stress, the second positive stress and the third positive stress can determine whether the wafer can be used. In the silicon carbide wafer of the present application, the difference between the first positive stress, the second positive stress and the third positive stress is not greater than 30MPa, that is, the stress of the wafer in the above three directions is uniformly distributed, and the mechanical properties of the wafer are more uniformly distributed.

[0010] Preferably, the difference between the first normal stress, the second normal stress and the third normal stress is no more than 20 MPa.

[0011] The first shear stress is a stress acting on the normal line of the X-axis and along the Y-axis direction, the second shear stress is a stress acting on the normal line of the Y-axis and along the Z-axis direction, and the third shear stress is a stress acting on the normal line of the Z-axis and along the X-axis direction. The above-mentioned first shear stress, second shear stress and third shear stress represent the ability of dislocation slip in the wafer product. The greater the shear stress, the more dislocations in the wafer will increase sharply during the processing of the wafer, which will lead to the failure of the device obtained by the wafer production. Therefore, the first shear stress, the second shear stress and the third shear stress can affect the performance of the wafer device. In the silicon carbide wafer of the present application, the difference between the first shear stress, the second shear stress and the third shear stress is not more than 20MPa, that is, the stress of the wafer in the above three directions is also uniformly distributed, and the dislocation slip can be weakened in any direction. Therefore, the device performance obtained using the wafer is also more uniform and stable.

[0012] Preferably, the difference between the first shear stress, the second shear stress and the third shear stress is no more than 15 MPa.

[0013] Preferably, the first normal stress, the second normal stress, the third normal stress, the first shear stress, the second shear stress and the third shear stress are uniformly distributed in the horizontal and vertical directions of the wafer, that is, the difference of each stress in the horizontal and vertical directions is relatively low.

[0014] According to another aspect of the present application, a method for non-destructively and accurately measuring the isotropic stress of a wafer is provided, comprising the following steps:

[0015] (1) performing an XRD diffraction test on the wafer, rotating the wafer in-plane and between planes during the test to obtain test results under at least 6 diffraction crystal planes, comparing the diffraction peaks of different diffraction crystal planes with the standard peaks of the corresponding diffraction crystal planes in the stress-free wafer to obtain the isotropic strain value of the wafer;

[0016] (2) Calculate the isotropic stress of the chip based on the isotropic strain value and elastic constant.

[0017] This test method is simple and uses a self-designed optimization algorithm to obtain accurate isotropic stress data of the wafer and the distribution of isotropic stress on the wafer surface.

[0018] Optionally, in step (1), the calculation formula of the strain value in each direction is:

[0019] ε xy =cos 2 αsin 2 β×ε 11 +sin2αsin 2 β×ε 12 +cosαsin2β×ε 13 +sin 2 αsin 2 β×ε 22 +sinαsin2β×ε 23 +cos2β×ε 33 Formula (1);

[0020] Among them, ε 11 is the first normal strain of the test point, ε 22 is the second normal strain of the test point, ε 33 is the third normal strain of the test point, ε 12 is the first shear strain at the test point, ε 23 is the second shear strain at the test point, ε 13 is the third shear strain of the test point, α is the in-plane rotation angle, β is the inter-plane rotation angle, and ε xy is the total strain value, and its calculation formula is:

[0021]

[0022] where d hkl is the actual interplanar spacing of any tested crystal plane, d 0 hkl is the theoretical interplanar spacing of any tested crystal plane.

[0023] To obtain the isotropic stress of the chip, you need to first obtain the isotropic strain value of the chip. The isotropic strain value of the chip is a second-order tensor expressed in the form of a 3×3 matrix. The matrix is ​​written as follows:

[0024]

[0025] ε 11 , ε 22 , ε 33 , ε 12 , ε 13 , ε 21 , ε 23 , ε 31 , ε 32 is the isotropic strain value at the test point, where ε 12 =ε 21 , ε 13 =ε 31 , ε 23 =ε 32 , so we only need to find ε 11 , ε 22 , ε 33 , ε 12 , ε 13 , ε 21 The value of can be used together with the elastic constant to calculate the isotropic stress of the chip.

[0026] In actual testing, different ε can be obtained for each diffraction crystal plane. xy value, so the above ε 11 , ε 22 , ε 33 , ε 12 , ε 13 , ε 23 is an unknown variable, so according to formula (1), the following equation can be constructed for the six diffraction crystal planes:

[0027]

[0028] In this formula:

[0029] cos 2 αsin 2 β=a 11 sin2αsin 2 β=a 12 cosasin2β=a 13

[0030] sin 2 αsin 2 β=a 14 sinαsin2β=a 15 cos2β=a 16 ,

[0031] For each diffraction crystal plane, its α and β are known, so a 11 、a 12、a 13 、a 14 、a 15 、a 16 is a known quantity, ε xy is a quantity that can be calculated based on the interplanar spacing. Based on the above known quantities, ε can be obtained. 11 , ε 22 , ε 33 , ε 12 , ε 13 , ε 23 The value of .

[0032] In the above calculation method, the elastic constant is an important parameter for studying the mechanical properties of materials. The elastic constant is a fourth-order tensor, and the writing method is relatively complicated. The specific parameters of the elastic constants of different wafers can be queried in the database. For hexagonal silicon carbide crystals, the elastic constant can be written in matrix form:

[0033]

[0034] Therefore, the calculation formula for the stress in each direction is:

[0035]

[0036] where σ 11 is the first normal stress at the test point, σ 22 is the second normal stress at the test point, σ 33 is the third normal stress at the test point, σ 12 is the first shear stress at the test point, σ 23 is the second shear stress at the test point, σ 13 is the third shear stress at the test point, C 66 =(C 11 -C 12 ) / 2,C 11 , C 12 , C 13 , C 33 and C 44 There are five independent parameters in the hexagonal crystal system.

[0037] The above formula can be used to calculate the isotropic stress of the wafer. The matrix expression of the isotropic stress is as follows:

[0038]

[0039] in

[0040] σ 12 =σ 21 , σ 32 =σ 23 , σ 13 =σ31 .

[0041] Optionally, there are at least 7 diffraction crystal planes.

[0042] The above stress values ​​refer to the absolute stress of the wafer at the test point, that is, the residual stress compared to the stress-free wafer. The first normal stress is the stress along the X-axis, the second normal stress is the stress along the Y-axis, the third normal stress is the stress along the Z-axis, and the first shear stress σ 12 is the stress acting on the normal line of the X-axis and along the Y-axis, and the stress acting on the normal line of the Y-axis and along the X-axis σ 21 Equal, the second shear stress σ 23 is the stress acting on the normal line of the Y axis and along the Z axis, and is the stress acting on the normal line of the Z axis and along the Y axis 32 Equal, the third shear stress σ 13 is the stress acting on the normal line of the X-axis and along the Z-axis direction, and the stress acting on the normal line of the Z-axis and along the X-axis direction σ 31 equal.

[0043] The above-mentioned structure constructed with 6 diffraction crystal planes contains ε 11 , ε 22 , ε 33 , ε 12 , ε 13 , ε 23 Detecting at least 7 diffraction crystal planes here can further improve the accuracy of the above-mentioned solutions of the isotropic strain values, thereby accurately determining the isotropic stress distribution of the chip.

[0044] Optionally, the diffraction crystal planes include (002) plane, (004) plane, (006) plane, (008) plane, (102) plane, (103) plane, (104) plane, (105) plane, (024) plane, (026) plane, (044) plane, (113) plane, (114) plane, and (115) plane.

[0045] Optionally, the peak intensity of the diffraction crystal plane is not less than 20,000 cps, and the half-width is not greater than 100 arcsec.

[0046] The diffraction intensity of the above-mentioned diffraction crystal plane is strong, and the half-width is moderate, which can scan the accurate information of the chip, so that a more accurate total strain value can be calculated. If the height and width of the diffraction crystal plane are greater than 100 arcsec, the detection accuracy of the chip will be reduced, and the total strain value obtained by the test will be unusable.

[0047] Optionally, the value range of α is 0-180°, and the value range of β is 0-90°. The chip can be rotated within the plane and between planes within the above range, so as to facilitate finding the required diffraction surface during the test process.

[0048] Optionally, in the XRD diffraction test, the penetration depth of XRD is 3-60 μm.

[0049] Optionally, the wafer is a silicon carbide wafer, and the silicon carbide wafer includes a semi-insulating type and a conductive type.

[0050] Optionally, the diameter of the wafer is greater than 6 inches, preferably 8 inches.

[0051] According to another aspect of the present application, a standard method for detecting isotropic stress of a wafer is provided, comprising the following steps:

[0052] Step 1: Place the wafer on the XRD test sample table, select the initial diffraction crystal plane, obtain the diffraction peak of the initial diffraction crystal plane, then rotate the wafer in-plane and between-planes to obtain diffraction peaks under at least 6 diffraction crystal planes, compare the diffraction peaks of the above diffraction crystal planes with the standard peaks of the corresponding diffraction crystal planes in the stress-free wafer, and obtain the total strain value ε under each diffraction crystal plane xy ;

[0053] Step 2: Calculate the isotropic strain value of the wafer according to the calculation formula of the total strain value and the isotropic strain value;

[0054] Step 3: Calculate the isotropic stress of the chip based on the isotropic strain values ​​calculated in the second step and the elastic constants of the chip.

[0055] In the standard method for detecting the isotropic stress of a wafer, the calculation formula for the isotropic strain value in the second step and the calculation formula for the isotropic stress in the third step are the same as the method for non-destructively and accurately measuring the isotropic stress of a wafer. The operator can calculate the isotropic stress of the wafer according to the steps and process of the above-mentioned standard method for detecting the isotropic stress of a wafer.

[0056] The beneficial effects of this application include but are not limited to:

[0057] 1. The current detection methods in the prior art are unable to distinguish and detect the normal stress and shear stress of the wafer. By adopting the method of non-destructively and accurately measuring the isotropic stress of the wafer of the present application, the magnitude of the isotropic stress at a certain test point on the wafer can be calculated by testing different diffraction crystal planes, thereby obtaining the isotropic stress distribution of the entire wafer.

[0058] 2. According to the method for non-destructively and accurately measuring the isotropic stress of a chip of the present application, the values ​​of the first normal strain, the second normal strain, the third normal strain, the first shear strain, the second shear strain and the third shear strain can be simplified and calculated according to the calculation formula of the isotropic strain, thereby calculating the isotropic stress value of the chip, providing a theoretical basis for the study of the isotropic stress of the chip.

[0059] 3. According to the method of non-destructively and accurately measuring the isotropic stress of a wafer in the present application, the test under different diffraction crystal planes is obtained by rotating the wafer in-plane and between-planes. The isotropic stress value of the test point can be obtained without destroying the wafer, which is suitable for industrial mass testing.

[0060] 4. According to the method for non-destructively and accurately measuring the isotropic stress of a wafer of the present application, the diffraction crystal plane provided can obtain a stronger diffraction peak in XRD diffraction, further improving the test accuracy of the method.

[0061] 5. According to the method of non-destructively and accurately measuring the isotropic stress of a wafer of the present application, the isotropic stress is calculated by using elastic constants, and the elastic constants of the fourth-order tensor are reasonably simplified mathematically, so that the calculation process is simpler and the calculation results are more accurate.

[0062] 6. According to the silicon carbide wafer of the present application, its first normal stress, second normal stress and third normal stress are approximately the same, the first shear stress, second shear stress and third shear stress are approximately the same, and the stress is uniformly distributed, which can prevent the wafer from slipping in all directions, thereby reducing the number of dislocations in the wafer, and improving the uniformity of dislocation distribution, reducing lattice distortion, and improving the stability and reliability of devices prepared from the wafer. BRIEF DESCRIPTION OF THE DRAWINGS

[0063] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0064] Figure 1 A top view of a fixture for wafer stress detection according to Embodiment 1 of the present application;

[0065] Figure 2 A side view of a fixture for wafer stress detection according to Embodiment 1 of the present application;

[0066] Figure 3 A top view of the permanent magnetic base involved in Example 1 of the present application;

[0067] Figure 4 A top view of the wafer to be tested according to Embodiment 1 of the present application;

[0068] Figure 5 A schematic diagram of XRD diffraction of a silicon carbide wafer according to Example 2 of the present application;

[0069] Figure 6 This is a diffraction result diagram of the silicon carbide wafer involved in Example 2 of the present application on the (004) plane;

[0070] Figure 7The diffraction result diagrams of the silicon carbide wafer involved in Example 2 of the present application at the (024), (114), (105), (102), (026), and (104) diffraction crystal planes respectively;

[0071] Figure 8 A schematic diagram of the directions of the various stresses of the silicon carbide wafer involved in Example 2 of the present application;

[0072] List of parts and reference numerals:

[0073] 1. Wafer to be tested; 2. Sample holder; 3. Sample placement plate; 4. Permanent magnetic base; 5. Sample stage; 6. Scale line; 7. Marking line. DETAILED DESCRIPTION

[0074] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0075] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.

[0076] Example 1

[0077] refer to Figure 1-4 The present embodiment discloses a fixture for wafer stress detection, comprising: a permanent magnetic base 4, a connecting component is provided at the bottom of the permanent magnetic base 4, and the connecting component is used to connect with a sample stage 5 of a detection instrument; a sample placement plate 3, the sample placement plate 3 is arranged above the permanent magnetic base 4, the sample placement plate 3 contains metal particles, and the sample placement plate 3 is used to place a wafer to be tested 1; a sample clamp 2, the sample clamp 2 is arranged above the sample placement plate 3, and the sample clamp 2 is circumferentially abutted against the wafer to be tested 1, and is used to clamp the wafer to be tested 1.

[0078] The permanent magnetic base 4 in the fixture is fixed on the sample stage 5 through a connecting component, so that the overall fixture is fixedly connected to the sample stage 5, thereby improving the stability of the overall fixture during testing. The metal particles arranged inside the sample placement plate 3 and the permanent magnetic base 4 are adsorbed by magnetic force, so that the sample placement plate 3 and the permanent magnetic base 4 are fixedly connected. The wafer 1 to be tested is placed on the sample placement plate 3 and fixed by the sample clamp 2. Therefore, under the cooperation of the sample placement plate 3 and the sample clamp 2, the fixture can replace the existing vacuum adsorption method to fix the wafer 1 to be tested during the stress detection process. No additional stress will be caused during the overall detection process, thereby ensuring the accuracy of stress detection of the wafer 1 to be tested. When the sample stage 5 is tilted to perform stress detection on the wafer 1 to be tested, the fixture can also clamp the wafer 1 to be tested, so that when the wafer 1 to be tested is subjected to in-plane and inter-plane rotation detection, the coordinates of the test point can still be guaranteed to remain unchanged.

[0079] Moreover, the sample placement plate 3 and the permanent magnetic base 4 are magnetically adsorbed, so that the position of the sample placement plate 3 on the permanent magnetic base 4 can be easily adjusted. Under this setting, the position of the wafer 1 to be tested can be adjusted without moving the sample stage 5, so as to realize stress detection of different positions of the wafer 1 to be tested, thereby improving the convenience of using the fixture.

[0080] As an embodiment, there are at least two sample clamps 2, and the side surfaces of the sample clamps 2 that abut against the wafer 1 to be tested are arc-shaped and are evenly arranged along the circumference of the wafer 1 to be tested. Under this arrangement, the wafer 1 to be tested can be evenly clamped and fixed in the circumference of the wafer 1 to be tested, thereby improving the stability of the fixture in use, and when testing wafers 1 to be tested of different sizes, the wafer 1 to be tested can be fixed again by replacing or moving a part of the sample clamps 2, thereby improving the adjustment flexibility of the fixture.

[0081] As an embodiment, the sample holder 2 contains metal particles inside, and the sample holder 2 can move along the upper surface of the sample placement plate 3. Under this setting, the sample placement plate 3 and the sample holder 2 are connected in a split type, and the position of the sample holder 2 on the sample placement plate 3 can be adjusted to clamp the wafers 1 to be tested of different sizes without replacing any parts, further improving the convenience and universality of the fixture.

[0082] As an embodiment, the permanent magnetic base 4 is made of neodymium iron boron material, and the thickness of the permanent magnetic base 4 and the sample placement plate 3 are both less than 3 mm. Since the fixture is fixed on the sample stage 5, the height of the entire fixture will not be too high. The permanent magnetic base 4 is made of neodymium iron boron material because it is easier to process into thin sheets, which can reduce the overall height of the fixture and facilitate the installation of the fixture on the sample stage 5 of the detection instrument.

[0083] As an implementation mode, the permanent magnetic base 4 is provided with scale lines 6, and the sample placement plate 3 is made of a transparent material. The scale lines 6 are provided on the permanent magnetic base 4, and the sample placement plate 3 is set to be a transparent material, so as to facilitate the positioning of the wafer 1 to be tested, improve the adjustment efficiency of the wafer 1 to be tested, and realize stress detection at different positions of the wafer 1 to be tested.

[0084] In actual use, such as Figure 3 As shown in FIG. 1 , it is a top view of the permanent magnetic base 4. The scale lines 6 are cross lines, and the intersection of the cross lines is the positioning point. Before the stress test is performed on the wafer 1 to be tested, a number of vertical marking lines 7 are drawn on its surface using a marker pen. The intersection of the marking lines 7 is the test point. Figure 4 As shown, during the test, the position of the sample placement plate 3 on the permanent magnetic base 4 is adjusted, and a certain test point of the wafer 1 to be tested is aligned and overlapped with a positioning point of the permanent magnetic base 4, so that the positioning of a certain test point can be achieved, and subsequent stress detection can be performed.

[0085] As a preferred embodiment, the sample placement plate 3 is made of polycarbonate or polymethyl methacrylate, the sample clamp 2 is made of polytetrafluoroethylene, and the connecting component is adhesive. The above arrangement can avoid scratches on the wafer 1 to be tested, and stably clamp the wafer 1 to be tested while ensuring safety.

[0086] Example 2

[0087] This embodiment relates to a method for processing a 6-inch silicon carbide wafer and a method for measuring stress in all directions:

[0088] 1. The processing method of silicon carbide wafer comprises the following steps:

[0089] (1) The cut silicon carbide wafer is annealed by raising the temperature to 1800°C, then the silicon carbide wafer is naturally cooled to room temperature in a heating furnace, and then ground with alumina with an average particle size of 1 μm for 5 hours. After grinding, the TTV of the silicon carbide wafer is less than 4 μm.

[0090] (2) Then, polishing is performed using silicon dioxide and cerium dioxide abrasives with a hardness lower than that of silicon carbide. The particle size of the two abrasives is 100 nm, and the weight ratio of silicon dioxide to cerium dioxide is 1:1. The mixing method is ball milling, and the polishing time is 3 to 5 hours to obtain a wafer with relatively uniform surface stress, and to completely remove the damaged layer on the surface of the wafer, eliminating the influence of non-elastic deformation. After polishing, the roughness of the silicon carbide wafer is less than 1 nm, or the TTV is less than 2 μm.

[0091] 2. The method for determining the stress in each direction includes the following steps:

[0092] (1) The ground or polished wafer is placed on the fixture in Example 1, and an XRD diffraction test is performed on the silicon carbide wafer. Figure 5 As shown in (a), the (004) plane with higher diffraction intensity is selected as the initial diffraction crystal plane. The diffraction results are shown in Figure 6 As shown, then Figure 5 As shown in (b), the wafer is rotated in-plane and between-planes to obtain diffraction peaks under the diffraction crystal planes of (024), (114), (105), (102), (026), and (104). The results are shown in Figure 7 As shown in the figure, the in-plane rotation angle α and the inter-plane rotation angle β of each diffraction crystal plane from the initial diffraction crystal plane are recorded, the diffraction peaks of the above 6 diffraction crystal planes are compared with the standard peaks of the corresponding diffraction crystal planes in the stress-free wafer, and the total strain values ​​ε of the 6 diffraction crystal planes are calculated according to the following formula: xy :

[0093]

[0094] where dhkl is the actual interplanar spacing of any tested crystal plane, d 0 hkl is the theoretical interplanar spacing of any tested crystal plane;

[0095] Substitute the 6 total strain values ​​obtained into the following formula:

[0096] ε xy =cos 2 αsin 2 β×ε 11 +sin2αsin 2 β×ε 12 +cosαsin2β×ε 13 +sin 2 αsin 2

[0097] β×ε 22 +sinαsin2β×ε 23 +cos2β×ε 33 ;

[0098] In the above formula, ε of each diffraction crystal plane is xy , α and β are known, they can be listed as seven equations, and ε can be calculated based on the seven equations 11 , ε 22 , ε 33 , ε 12 , ε 13 , ε 23 The value of ε 11 , ε 22 , ε 33 , ε 12 , ε 13 , ε 23 It is the isotropic strain value of the chip.

[0099] (2) Calculate the isotropic stress of the wafer based on the isotropic strain value and the elastic constant. The calculation formula is as follows, where the elastic constant queries the parameters in the database:

[0100]

[0101] In the above stress matrix, the directions of the stresses expressed by the parameters are as follows: Figure 8 As shown, σ 11 , σ 22 , σ 33 is the normal stress, and the other components are shear stresses. The obtained stress results in various directions are shown in Table 1 below. The center point of the chip in Table 1 is the coordinate (0,0).

[0102] Table 1

[0103]

[0104] Example 3

[0105] The present embodiment relates to a method for processing an 8-inch silicon carbide wafer and a method for measuring stress in various directions. The steps in the processing method and the measuring method are the same as those in Example 2. The stress data of the 8-inch silicon carbide wafer in various directions are obtained. The results are shown in Table 2 below. In Table 2, the center point of the wafer is the coordinate (0, 0).

[0106] Table 2

[0107]

[0108] Reliability Verification

[0109] The reliability of the silicon carbide wafer tested by the method for measuring the stress in each direction in the above-mentioned embodiment 2 and embodiment 3 is verified, specifically: using an X-ray diffractometer with different wavelengths to verify the reliability of the strain test, and then obtain a feasibility analysis of the stress test. The strain value tested with the Cu target is recorded as The strain value measured by Mo target is recorded as pass The reliability is determined by comparing the difference between the two. In the determination method of the present application, Δ is less than 1%, which proves that the determination method of the stress in each direction of the present application has high reliability and accuracy.

[0110] The above is only the embodiment of the present application, and the protection scope of the present application is not limited by these specific embodiments, but is determined by the claims of the present application. For those skilled in the art, the present application can have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the technical ideas and principles of the present application should be included in the protection scope of the present application.

Claims

1. A method for non-destructively and accurately measuring the isotropic stress of a wafer, characterized in that: The steps include: (1) Perform an XRD diffraction test on the wafer, select the initial diffraction crystal plane, obtain the diffraction peak of the initial diffraction crystal plane, then rotate the wafer in-plane and between-planes to obtain diffraction peaks under at least 6 diffraction crystal planes, compare the diffraction peaks of the above diffraction crystal planes with the standard peaks of the corresponding diffraction crystal planes in the stress-free wafer, and obtain the total strain value ε under each diffraction crystal plane xy , and its calculation formula is: , where d hkl is the actual interplanar spacing of any tested crystal plane, d 0 hkl is the theoretical interplanar spacing of any tested crystal plane; (2) According to the total strain value ε xy The isotropic strain value of the wafer is obtained by using the calculation formula of the isotropic strain value, the peak intensity of the diffraction crystal plane is not less than 20000cps, and the half-height width is not greater than 100arcsec. The calculation formula of the isotropic strain value is: e xy =cos 2 asin 2 b×e 11 +sin2αsin 2 b×e 12 +cosαsin2β×ε 13 +sin 2 asin 2 b×e 22 +sinαsin2β×ε 23 +cos2β×ε 33 ; Among them, ε 11 is the first normal strain of the test point, ε 22 is the second normal strain of the test point, ε 33 is the third normal strain of the test point, ε 12 is the first shear strain at the test point, ε 23 is the second shear strain at the test point, ε 13 is the third shear strain of the test point, α is the in-plane rotation angle, the value range of α is 0-180°, β is the inter-plane rotation angle, the value range of β is 0-90°, (3) Based on the calculated isotropic strain values ​​and elastic constants, calculate the isotropic stress of the chip.

2. The method according to claim 1, characterized in that: The calculation formula for the stress in each direction is: , where σ 11 is the first normal stress at the test point, σ 22 is the second normal stress at the test point, σ 33 is the third normal stress at the test point, σ 12 is the first shear stress at the test point, σ 23 is the second shear stress at the test point, σ 13 is the third shear stress at the test point, C 66 =(C 11 -C 12 ) / 2, C 11 , C 12 , C 13 , C 33 and C 44 There are five independent parameters in the hexagonal crystal system.

3. The method according to claim 1 or 2, characterized in that: The diffraction crystal planes include (002) plane, (004) plane, (006) plane, (008) plane, (102) plane, (103) plane, (104) plane, (105) plane, (024) plane, (026) plane, (044) plane, (113) plane, (114) plane, and (115) plane.

4. The method according to claim 1 or 2, characterized in that: In the XRD diffraction test, the penetration depth of XRD is 3-60 μm.

5. A silicon carbide wafer with uniformly distributed stress, characterized in that: The isotropic stress of the silicon carbide wafer is obtained by testing using the method as claimed in claim 1, wherein the first normal stress, the second normal stress and the third normal stress of the silicon carbide wafer are all less than 60 MPa, and the difference between the first normal stress, the second normal stress and the third normal stress is less than 30 MPa; The first shear stress, the second shear stress and the third shear stress of the silicon carbide wafer are all no greater than 30 MPa, and the difference between the first shear stress, the second shear stress and the third shear stress is no greater than 20 MPa.