Ultra-low temperature sintered glass-ceramics and preparation method and application thereof
By using Li2O, B2O3 and Al2O3 in specific component ratios in microcrystalline glass, ultra-low temperature sintering is achieved, and the problems of poor dielectric properties and reaction with electrodes are solved, and microcrystalline glass with excellent dielectric properties at high frequency are prepared. , suitable for LTCC substrate materials.
Patent Information
- Application Number
- CN202310740472.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-20
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-06-20
AI Technical Summary
The existing microcrystalline glass has poor dielectric performance during sintering, especially under ultra-low temperature sintering conditions, and may react with aluminum and silver electrodes, limiting its application in electronic devices.
Microcrystalline glass with a component ratio of 48-52 mol% Li2O, 43-47 mol% B2O3 and 3-7 mol% Al2O3 was prepared by melting, water quenching, crushing and pressing, so as to achieve ultra-low temperature sintering and the main crystal phase. It is LiBO2 and the secondary crystal phase is Li3AlB2O6. It can be sintered at 650°C to separate the sintering and crystallization processes, and improve density and dielectric properties.
A microcrystalline glass with high thermal expansion coefficient, low dielectric constant and low dielectric loss at 12.5~13.6GHz frequency is realized. It can be co-fired with aluminum or silver electrodes, meet the needs of LTCC substrate materials, and improve the small size of electronic devices. , lightweight and multifunctional capabilities.
Smart Images

Figure CN116693200B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of low-temperature co-fired ceramics, and in particular relates to an ultra-low temperature sintered microcrystalline glass and a preparation method and application thereof. Background Art
[0002] Low Temperature Co-fired Ceramic (LTCC) is a material used in the electronics industry that has excellent electrical, mechanical and thermal properties. In recent years, with the development of miniaturization and integration of electronic devices, this material has been widely studied due to its ability to integrate multiple components into a single packaged device. The main technical routes are: ceramic LTCC, microcrystalline glass LTCC and glass + ceramic composite LTCC. LTCC is a multilayer ceramic material manufactured at relatively low temperatures, usually less than 900°C; it has good dielectric properties at high frequencies, making it an ideal material for integrating metal conductors, resistors, capacitors and other components. As the demand for smaller and more efficient devices continues to increase, LTCC is likely to become an increasingly important material in the electronics industry.
[0003] In the past, LTCC was fired at temperatures ranging from 850°C to 1000°C, which limited its use in certain types of electronic devices. The development of LTCC ultra-low temperature sintering technology has been achieved with the adoption of new materials and processes. ULTCC technology utilizes a co-firing process that allows the integration of multiple layers of circuits, capacitors, resistors, and other components on a single substrate, making it an ideal solution for the miniaturization of electronic devices. Compared with traditional electronic packaging methods, ULTCC technology has several advantages, including high reliability, excellent electrical and thermal performance, and low cost. The development of ultra-low temperature sintering technology has also made LTCC more environmentally friendly. Lower firing temperatures reduce energy consumption and carbon emissions associated with the manufacturing process. But there are currently few ultra-low temperature sintered microcrystalline glass with high frequency and high dielectric properties.
[0004] The key defect of microcrystalline glass materials in the preparation of ULTCC materials is the deterioration of the dielectric properties of microglass, especially the increase in dielectric loss. The main reason for the deterioration of performance is the glass phase introduced during the sintering process to reduce the sintering temperature. After the sintering process is completed, under the premise of ensuring density, the glass phase is crystallized or secondary crystallized to reduce the glass phase and improve the dielectric properties of microglass, which is another key issue in the development of LTCC technology. In addition, some microcrystalline glass that is sintered densely may also react with aluminum and silver electrodes, thereby limiting its application in practice. Therefore, the development of a new type of microcrystalline glass LTCC material with ultra-low sintering temperature and low cost, which can be co-fired with common electrodes such as aluminum and silver, is of great significance to the miniaturization, lightweight and multifunctionality of electronic devices. Summary of the invention
[0005] The purpose of the present invention is to overcome the above-mentioned technical deficiencies, provide a microcrystalline glass sintered at an ultra-low temperature and a preparation method and application thereof, and solve the technical problem in the prior art that the microcrystalline glass sintering temperature is too high or the ultra-low temperature sintering leads to poor dielectric properties.
[0006] In order to achieve the above technical purpose, the technical solution provided by the present invention is:
[0007] In a first aspect, the present invention provides an ultra-low temperature sintered glass-ceramics, which comprises the following components, calculated by molar percentage of oxides: 48-52 mol% Li2O, 43-47 mol% B2O3 and 3-7 mol% Al2O3.
[0008] In a second aspect, the present invention provides a method for preparing ultra-low temperature sintered microcrystalline glass, comprising the following steps: weighing raw materials according to the component ratio, mixing them evenly to obtain a mixture; melting the mixture and quenching it with water to obtain glass slag, and then drying the glass slag and crushing and sieving it to obtain glass powder; pressing the glass powder into shape to obtain a glass green body, and then keeping the glass green body at 610-650°C for 3-10 hours and then cooling it to room temperature to obtain ultra-low temperature sintered microcrystalline glass.
[0009] In a second aspect, the present invention provides an application of ultra-low temperature sintered glass-ceramics in the preparation of an ultra-low temperature co-fired ceramic substrate.
[0010] Compared with the prior art, the beneficial effects of the present invention include:
[0011] (1) The preparation method of the present invention is simple and reasonable. By rationally configuring the composition of various raw materials, the sintering process and the crystallization process of the glass-ceramics are separated, so that the prepared glass-ceramics have a lower sintering temperature and a higher sintering densification.
[0012] (2) The glass-ceramics with ultra-low sintering temperature (650°C) prepared by the present invention has a high thermal expansion coefficient (13-15ppm / °C), a low dielectric constant (5.5-7.5) and a low dielectric loss (0.00062-0.00285) at a frequency of 12.5-13.6GHz, and has good dielectric properties; at the same time, it can be co-sintered with aluminum or silver electrodes to meet the application requirements of LTCC substrate materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 These are SEM photos of the microcrystalline glass described in Example 1 after co-firing with a silver electrode and an aluminum electrode, and line scanning analysis diagrams of interface elements.
[0014] Figure 2 XRD patterns of the ultra-low temperature sintered glass-ceramics described in Examples 1 to 10. DETAILED DESCRIPTION
[0015] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0016] The invention provides ultra-low temperature sintered microcrystalline glass and a preparation method and application thereof.
[0017] In the first aspect, the present invention provides an ultra-low temperature sintered glass-ceramics, which comprises the following components, calculated by molar percentage of oxides: 48-52 mol% Li2O, 43-47 mol% B2O3, and 3-7 mol% Al2O3; the main crystalline phase of the ultra-low temperature sintered glass-ceramics is LiBO2, and the secondary crystalline phase is Li3AlB2O6.
[0018] Preferably, the following components are included, calculated by molar percentage of oxides: 48-52 mol% Li2O, 43-47 mol% B2O3, and 4-5 mol% Al2O3.
[0019] In a second aspect, the present invention provides a method for preparing ultra-low temperature sintered glass-ceramics, comprising the following steps:
[0020] (1) weighing raw materials according to the component ratio, mixing them to obtain slurry, and finally drying the slurry to obtain a mixture;
[0021] (2) keeping the mixture in step (1) at 900-1100° C. for 5-15 minutes, taking it out, and quenching it with water to obtain glass slag; drying the glass slag, ball milling it, and sieving it to obtain glass powder;
[0022] (3) The glass powder of step (2) is sieved and pressed into a glass green body, which is then kept at 610-650° C. for 3-10 hours and then cooled to room temperature to obtain the ultra-low temperature sintered microcrystalline glass.
[0023] Preferably, the mixing method of step (1) is: raw material: grinding medium: anhydrous ethanol = 1:5:2 by mass ratio is put into a mixing tank and mixed for 8 to 16 hours, more preferably 10 to 14 hours.
[0024] Preferably, the grinding medium is a zirconia ball with a diameter of 1 mm to 40 mm.
[0025] Preferably, the drying temperature in step (1) is 60-90° C., and the drying time is 4-6 hours; more preferably, the drying is performed at 80° C. for 5 hours.
[0026] Preferably, the mixture in step (2) is kept at 1000° C. for 10 minutes.
[0027] Preferably, the mesh number of the sieving in step (2) is ≥20 mesh, for example, 20 mesh, 40 mesh, 60 mesh, 80 mesh, 100 mesh, 120 mesh, 140 mesh, 160 mesh, 180 mesh, 200 mesh, 230 mesh or 270 mesh, etc.
[0028] Preferably, the drying temperature in step (2) is 60-90° C., and the drying time is 10-14 h; more preferably, the drying is performed at 80° C. for 12 h.
[0029] Preferably, the ball milling method in step (2) is: glass slag: grinding medium: anhydrous ethanol = 1:5:2 is loaded into a ball mill and ball milled for 2 to 6 hours to obtain glass powder; the grinding medium is a zirconia ball with a diameter of 1 mm to 40 mm.
[0030] Preferably, the mesh size of the sieving in step (3) is 200 meshes.
[0031] Preferably, the pressing pressure in step (3) is 5 to 20 MPa.
[0032] Preferably, in step (3), the glass powder is sieved and then pressed for 5-15 minutes to obtain a glass green body (if the holding time is too short, the contact between the glass powders will be insufficient and affect the subsequent sintering; if the holding time is too long, the glass green body may be deformed during the sintering process); then the temperature is raised to 610-650°C at a rate of 5°C / min, kept at this temperature for 3-10 hours, and then naturally cooled to room temperature to obtain the ultra-low temperature sintered microcrystalline glass.
[0033] More preferably, in step (3), the temperature is kept at 630-650° C. for 4-10 h, more preferably at 650° C. for 5-7 h.
[0034] In a third aspect, the present invention further provides an application of ultra-low temperature sintered glass-ceramics in the preparation of ultra-low temperature co-fired ceramic substrates.
[0035] The present invention is further described in detail below through specific examples.
[0036] Example 1
[0037] A method for preparing ultra-low temperature sintered glass-ceramics, comprising the following steps:
[0038] (1) Various oxide raw materials are prepared according to the composition of Li2O: 50 mol%; B2O3: 46 mol%; Al2O3: 4 mol%. Raw materials: zirconium oxide balls: anhydrous ethanol = 1:5:2 are placed in a mixing tank and mixed for 12 hours to obtain a uniform mixed slurry, which is placed in an oven at 80°C for 5 hours for drying;
[0039] (2) the dried mixture is placed in a platinum crucible, placed in a lifting furnace at 1000° C. for 10 min, taken out, poured into deionized water for quenching to obtain glass slag; placed in an oven at 80° C. for 12 h for drying, and placed in a ball mill according to the ratio of raw material: zirconium oxide ball: anhydrous ethanol = 1:5:2 for ball milling for 4 h to obtain glass powder;
[0040] (3) After passing the glass powder through a 200-mesh sieve, pressing the glass powder under a pressure of 20 MPa for 10 minutes to obtain a glass green body; placing the glass green body into a sintering furnace, keeping it at 650° C. for 7 hours, and then cooling it to room temperature to obtain the microcrystalline glass.
[0041] The dielectric constant and loss of glass-ceramics were measured at 13.6 GHz using an LCR meter (Agilent 4292A, USA). The test results are as follows: r =5.5, dielectric loss tanθ=6.2×10 -4 , coefficient of thermal expansion CTE = 14.0ppm / ℃.
[0042] Example 2
[0043] The only difference between Example 2 and Example 1 is that the insulation time is changed to 3 hours, and the other steps and conditions are the same as those of Example 1.
[0044] The dielectric constant and loss of glass-ceramics were measured at 13.6 GHz using an LCR meter (Agilent 4292A, USA). The test results are as follows: r =5.4,tanθ=1×10 -3 , CTE = 14.2ppm / ℃.
[0045] Example 3
[0046] The only difference between Example 3 and Example 1 is that the insulation time is changed to 4 hours, and the other steps and conditions are the same as those of Example 1.
[0047] The dielectric constant and loss of glass-ceramics were measured at 12.5 GHz using an LCR meter (Agilent 4292A, USA). The test results are as follows: r =7.3,tanθ=8.5×10 -4 , CTE = 13.8ppm / ℃.
[0048] Example 4
[0049] The only difference between Example 4 and Example 1 is that the insulation time is changed to 5 hours, and the other steps and conditions are the same as those of Example 1.
[0050] The dielectric constant and loss of glass-ceramics were measured at 12.5 GHz using an LCR meter (Agilent 4292A, USA). The test results are as follows: r =7.3,tanθ=7.0×10 -4 , CTE = 14.5ppm / ℃.
[0051] Example 5
[0052] The only difference between Example 5 and Example 1 is that the insulation time is changed to 10 hours, and the other steps and conditions are the same as those in Example 1.
[0053] The dielectric constant and loss of glass-ceramics were measured at 12.5 GHz using an LCR meter (Agilent 4292A, USA). The test results are as follows: r =7.5,tanθ=8.2×10 -4 , CTE = 14.2ppm / ℃.
[0054] Example 6
[0055] The only difference between Example 6 and Example 2 is that the insulation temperature is changed to 630°C, and the other steps and conditions are the same as Example 2.
[0056] The dielectric constant and loss of glass-ceramics were measured at 13 GHz using an LCR meter (Agilent 4292A, USA). The test results are as follows: r =6.5,tanθ=2.85×10 -3 , CTE = 13.6ppm / ℃.
[0057] The main conditions and test results of the above embodiments 1-6 are statistically analyzed, and the results are shown in Table 1 below.
[0058] Table 1 Main conditions and test results of Examples 1-6
[0059]
[0060] It can be seen from Examples 1-5 that with the increase of the holding time, the contents of the main crystalline phase and the secondary crystalline phase both increase, wherein the main crystalline phase mainly provides a lower dielectric constant, and the secondary crystalline phase mainly provides a lower dielectric loss; and the XRD diffraction peak intensity increases significantly when the holding time is 4 hours, so the preferred holding time of the present invention is 3 to 10 hours, and more preferably 4 to 10 hours.
[0061] It can be seen from Example 2 and Example 6 that as the insulation temperature decreases, the XRD diffraction peak is weaker, the growth of the crystalline phase is not sufficient, and a large amount of glass phase exists, which reduces the dielectric properties of the microcrystalline glass.
[0062] Examples 7-10
[0063] The difference between Examples 7-10 and Example 2 is that the component ratio is adjusted, the other steps and conditions are the same as Example 2, and the total content of Al2O3 and B2O3 is 50 mol%. The specific ratio and the test results of the obtained microcrystalline glass are shown in Table 2 below.
[0064] Table 2 Main conditions and test results of Examples 7-10
[0065]
[0066] It can be seen from Example 9 and Example 2 that the dielectric properties of the microcrystalline glass decrease when the Al2O3 content increases to 6 mol%, which is related to the excessive growth of the crystals due to the excessive Al2O3.
[0067] Performance Testing
[0068] Take the glass powder in Example 1 and add 20wt% Ag powder or 20wt% Al powder, mix well and press at 20MPa pressure for 10min to obtain a mixed green body; put the green body into a sintering furnace, keep it at 650℃ for 7h and then cool it to room temperature to obtain a co-fired sample. After polishing the cross section of the sample, use a scanning electron microscope (SEM, Joel, JSM-7500F) equipped with an energy dispersive spectrometer (EDS, X-max N80) to test the cross section SEM photos.
[0069] Figure 1 These are SEM photographs and line scanning analysis diagrams of interface elements of the microcrystalline glass described in Example 1 after co-firing with a silver electrode and an aluminum electrode, respectively, wherein (a) corresponds to the SEM photograph and line scanning analysis diagram of interface elements of Example 1 after co-firing with a silver electrode; (b) corresponds to the SEM photograph and line scanning analysis diagram of interface elements of Example 1 after co-firing with an aluminum electrode.
[0070] from Figure 1 As can be seen from (a) and (b), the glass-ceramic is tightly bonded to the silver electrode or the aluminum electrode. There is a clear interface between the glass-ceramic and the electrode without an obvious transition layer. Element line scanning confirms that the silver and aluminum electrodes do not diffuse during the co-firing process and do not chemically react with the glass powder.
[0071] Figure 2 The XRD patterns of the ultra-low temperature sintered glass-ceramics described in Examples 1 to 10 are as follows: Figure 2It can be seen that the main crystalline phase of the microcrystalline glass prepared in Examples 1 to 10 is LiBO2. The peak intensity of Examples 2 and 6 is not high, indicating that the degree of crystallization is not high, and the final macroscopic performance is slightly reduced, so the insulation temperature cannot be too low and the insulation time cannot be too short. Compared with Example 8, the dielectric properties of Examples 2, 7, 9, and 10 have all decreased, showing a trend of first increasing and then decreasing, indicating that it is necessary to select a suitable Al2O3 content. Too much or too little Al2O3 will reduce the dielectric properties.
[0072] Similarly, through SEM photos and interface element line scanning tests, it can be obtained that the ultra-low temperature sintered microcrystalline glass prepared in Examples 2 to 6 does not diffuse during the co-firing process with the silver and aluminum electrodes, and does not chemically react with the glass powder.
[0073] Compared with the prior art, the present invention discloses an ultra-low temperature sintered glass-ceramics and a preparation method thereof and its application in ULTCC. The glass-ceramics comprises the following components in terms of molar percentage of oxides: 48-52 mol% Li2O, 43-47 mol% B2O3, and 3-7 mol% Al2O3; the main crystalline phase obtained by the glass-ceramics under ultra-low temperature sintering is LiBO2; the ultra-low sintering temperature is 650°C. In this composition, Li2O and B2O3 mainly form the crystalline phase LiBO2, and the addition of a large amount of alkali metals enables it to melt at a lower temperature (~1000°C). The addition of Al2O3 can increase the density, reduce the sintering shrinkage temperature, and regulate the size of the grains. The glass-ceramics has a high thermal expansion coefficient (13-15 ppm / °C), a low dielectric constant (5.5-7.5) and a low dielectric loss (0.00062-0.00285) at a frequency of 13.6 GHz. It has lower dielectric loss at high frequencies and can be co-fired with aluminum or silver electrodes. It can be applied to ULTCC substrates and electronic sealing materials.
[0074] The specific implementation of the present invention described above does not constitute a limitation on the protection scope of the present invention. Any other corresponding changes and modifications made based on the technical concept of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A method for preparing ultra-low temperature sintered glass-ceramics, characterized in that: The glass-ceramics comprises the following components, calculated by molar percentage of oxides: 50 mol % of Li2O, 46 mol % of B2O3 and 4 mol % of Al2O3; The method for preparing the microcrystalline glass comprises the following steps: Weigh the raw materials according to the group distribution ratio, and mix them evenly to obtain a mixed material; The mixed material is melted and then quenched to obtain glass slag, which is then dried and crushed to obtain glass powder; the melting conditions of the mixed material are: keeping the temperature at 1000° C. for 10 minutes; After the glass powder is passed through a 200-mesh sieve, it is pressed at a pressure of 20 MPa for 10 minutes to obtain a glass green body. The glass green body is kept at 650°C for 7 hours and then cooled to room temperature to obtain ultra-low temperature sintered microcrystalline glass. At a frequency of 13.6 GHz, the thermal expansion coefficient of glass-ceramics is 14 ppm / °C, the dielectric constant is 5.5, and the dielectric loss is 0.00062.
2. The method for preparing ultra-low temperature sintered glass-ceramics according to claim 1, characterized in that: The main crystalline phase of the ultra-low temperature sintered glass-ceramics is LiBO2, and the secondary crystalline phase is Li3AlB2O6.
3. The method for preparing ultra-low temperature sintered glass-ceramics according to claim 1, characterized in that: The raw materials are mixed evenly by ball milling for 12 hours and then drying to obtain the mixed material.
4. The method for preparing ultra-low temperature sintered glass-ceramics according to claim 1, characterized in that: The glass slag is dried at 80° C. and pulverized by ball milling for 4 hours.
5. The method for preparing ultra-low temperature sintered glass-ceramics according to claim 1, characterized in that: The heating rate of the glass green body is 5° C. / min.
6. Use of the ultra-low temperature sintered glass-ceramics obtained by the preparation method according to any one of claims 1 to 5 in the preparation of ultra-low temperature co-fired ceramic substrates.