A method for recovering nickel-cobalt-manganese-oxide lithium waste by wet method

By utilizing multiple cycle reactions and hot-melt freezing methods in the wet process, combined with sodium hydroxide to adjust pH, the problem of lithium loss in the wet process is solved, the recovery rate of lithium is improved, and the process cost is reduced, achieving high efficiency. , environmentally friendly valuable metal recycling.

CN116694933BActive Publication Date: 2024-10-01GANSU RUISIKE NEW MATERIAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310951877.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-31
Publication Date
2024-10-01
Estimated Expiration
2043-07-31

AI Technical Summary

Technical Problem

The existing wet process uses a large amount of organic solvents when recycling lithium nickel cobalt manganate waste, causing environmental pollution and producing a large amount of sodium sulfate decahydrate, resulting in the loss of lithium.

Method used

After calcining the lithium nickel cobalt manganate waste, concentrated sulfuric acid, hydrogen peroxide and pure water are used to carry out multiple circulation reactions, combined with hot melting and freezing methods, to separately precipitate manganese sulfate and cobalt sulfate, nickel sulfate mixed crystals, and use sodium hydroxide to adjust the pH , reduce the production of sodium sulfate decahydrate and improve the recovery rate of lithium.

Benefits of technology

The loss of lithium is significantly reduced, the recovery rate of lithium is improved, the process cost is reduced, and the safety and environmental problems caused by the use of large amounts of organic solvents and sodium hydroxide are avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_10
    Figure SMS_10
  • Figure SMS_11
    Figure SMS_11
Patent Text Reader

Abstract

The invention discloses a method for wet-process recovery of nickel-cobalt-manganese-oxide waste, which belongs to the field of waste lithium battery recovery and solves the problem of lithium loss in the existing wet process. The method of the invention is as follows: after calcining the nickel-cobalt-manganese-oxide waste, concentrated sulfuric acid, hydrogen peroxide and pure water are added, and leaching solution I is filtered to obtain; after the leaching solution I is heated, the calcined material, hydrogen peroxide and concentrated sulfuric acid are added, and leaching solution II is filtered to obtain; the leaching solution II is heated, filtered to obtain manganese sulfate crystals and leaching solution III, and the leaching solution III is cooled to obtain cobalt sulfate and nickel sulfate mixed crystals and leaching solution IV; the leaching solution IV repeats the above operation, and when the lithium content in the leaching solution is enriched, sodium hydroxide is added, and ternary precursors and lithium sulfate solutions are obtained by filtering; after the lithium sulfate solution is carbonized, sulfuric acid is added, and freezing treatment is performed, and sodium sulfate decahydrate and lithium sulfate solutions without sodium sulfate are obtained by filtering. The invention uses a method combining hot melting and freezing to recover valuable metal lithium in the crystal water of sodium sulfate decahydrate, thereby reducing lithium loss.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of waste lithium battery recycling, and specifically relates to a method for wet recycling of nickel-cobalt-manganese-lithium oxide waste. Background Art

[0002] With the rapid development of the lithium battery industry, more and more waste lithium batteries are generated, resulting in waste of resources and environmental pollution. Therefore, it is of great significance to recycle the valuable metals in waste lithium batteries. At present, there are mainly pyrolysis and hydrolysis in the treatment of positive electrode materials of nickel cobalt manganese oxide. In the wet recovery, the valuable metals are prepared into cobalt sulfate, manganese sulfate, and cobalt sulfate by solvent extraction. When the solvent extraction method recovers nickel, cobalt, and manganese, it is necessary to saponify the solvent first, and then strip it to obtain cobalt sulfate, manganese sulfate, and cobalt sulfate. This method requires the use of a large amount of organic solvents, the production process is complicated, and it is easy to cause environmental pollution and produce a large amount of sodium sulfate decahydrate to take away the valuable metal lithium. Summary of the invention

[0003] The purpose of the present invention is to provide a method for wet recovery of nickel-cobalt-manganese-lithium oxide waste, so as to solve the problem that the existing wet process uses a large amount of organic solvent and produces a large amount of sodium sulfate decahydrate, resulting in lithium loss.

[0004] The technical solution of the present invention is: a method for wet recovery of nickel-cobalt-manganese-lithium oxide waste, comprising the following steps:

[0005] A. calcining nickel-cobalt-lithium manganate waste under air flow to obtain a calcined material;

[0006] B. Add concentrated sulfuric acid, hydrogen peroxide and pure water to the calcined material obtained in step A, raise the temperature to 80-90° C., react for 1-3 hours, separate the solid and liquid to obtain leached residue I and leached solution I, wherein the concentration of manganese in the leached solution I is 85-90 g / L, and the total concentration of nickel and cobalt is 200-210 g / L. After filtering, the temperature of the leached solution I is maintained at 60-70° C.;

[0007] C. The leachate I obtained in step B is heated to 65-70° C., and then the calcined material, hydrogen peroxide and concentrated sulfuric acid are added, the reaction time is 1-3h, and the temperature of the filtered liquid is maintained at 60-65° C. to obtain leachate II and leach residue II, wherein the concentration of manganese in the leachate II is 170-180g / L, and the total concentration of cobalt and nickel is 400-420g / L; the leachate II is heated to not less than 95° C., solid-liquid separation is performed while hot, and the temperature of the filtered liquid is maintained at 90-95° C. to obtain manganese sulfate crystals and leachate III, and the temperature of the leachate III is further reduced to 25-30° C. to obtain mixed crystals of cobalt sulfate and nickel sulfate and leachate IV;

[0008] D. Raise the temperature of the leachate IV to 65-70° C., add the calcined material, hydrogen peroxide and concentrated sulfuric acid, repeat the operation of step C, and repeat the operation continuously to continuously precipitate manganese sulfate crystals and mixed crystals of cobalt sulfate and nickel sulfate; during the repetitive process, when the lithium content in the leachate is enriched to 20-25 g / L, stop adding the material, raise the temperature of the leachate to not less than 90° C., add sodium hydroxide to adjust the pH to 11-12, and separate the solid and liquid to obtain a ternary precursor and a lithium sulfate solution;

[0009] E. Adding sodium carbonate to the lithium sulfate solution obtained in step D to react, and separating the solid and liquid to obtain lithium carbonate and carbonized liquid;

[0010] F. After carbonization, sulfuric acid is added to the liquid to adjust the pH to 5-6, and then the liquid is frozen at a temperature of -10-0°C for 30-60 minutes. The solid-liquid separation is performed to obtain sodium sulfate decahydrate and a lithium sulfate solution free of sodium sulfate.

[0011] As a further improvement of the present invention, in step A, the calcination temperature is 600-700° C., and the calcination time is 1-3 h.

[0012] As a further improvement of the present invention, in step E, the reaction time is 40-60 min, and the reaction temperature is 90-100°C.

[0013] As a further improvement of the present invention, in step E, the amount of sodium carbonate used is 9-9.5 times the mass of the total lithium in the lithium sulfate solution.

[0014] As a further improvement of the present invention, in step F, the obtained lithium sulfate solution free of sodium sulfate is returned to step B for further leaching.

[0015] As a further improvement of the present invention, in step F, the obtained sodium sulfate decahydrate is subjected to heat melting treatment, and the volume is evaporated and concentrated to 1 / 3-1 / 2 of the original volume, and the solid-liquid separation is performed while hot to obtain the lithium-containing solution and glauber salt.

[0016] As a further improvement of the present invention, in step F, phosphoric acid is added to the obtained lithium-containing solution, and sodium hydroxide is added to adjust the pH to 10-11 to prepare lithium phosphate.

[0017] As a further improvement of the present invention, in step F, when preparing lithium phosphate, the reaction temperature is not less than 90° C., and the reaction time is 40-60 min.

[0018] As a further improvement of the present invention, in step F, when preparing lithium phosphate, the amount of phosphoric acid used is 1.04-1.05 times the theoretical amount.

[0019] The beneficial effects of the present invention are:

[0020] The present invention ingeniously utilizes the characteristics of different solubility of nickel sulfate, cobalt sulfate and manganese sulfate with increasing temperature. The solubility of cobalt sulfate and nickel sulfate increases with increasing temperature, while the solubility of manganese sulfate first increases and then decreases with increasing temperature. Manganese sulfate and cobalt sulfate and nickel sulfate have different saturations at the same temperature, so that manganese sulfate and cobalt sulfate and nickel sulfate reach their respective supersaturation points. After the temperature changes, supersaturation is utilized to crystallize and precipitate manganese sulfate and mixed crystals of cobalt sulfate and nickel sulfate. Multiple cycles of feeding can continuously precipitate manganese sulfate and mixed crystals of cobalt sulfate and nickel sulfate. The present invention uses a method combining hot melting and freezing to recover valuable metal lithium in the by-product sodium sulfate decahydrate crystal water, greatly reducing lithium loss.

[0021] The present invention uses sodium hydroxide only after lithium is enriched to 20-25 g / L when recovering valuable metals nickel, cobalt, manganese and lithium. Very little sodium sulfate decahydrate is produced, so that the amount of valuable metal lithium that can be taken away by the sodium sulfate decahydrate is very small, and the recovery rate of lithium is high. The present invention does not use a large amount of organic solvents and uses a small amount of sodium hydroxide compared to the traditional process, so the recovery cost is greatly reduced.

[0022] The invention is simple and easy to operate. Compared with the traditional solvent extraction process for recovering sulfate, the invention has a simple process and avoids the use of a large amount of organic solvents and sodium hydroxide to cause safety and environmental accidents. DETAILED DESCRIPTION

[0023] The present invention is described in detail below in conjunction with specific implementation modes.

[0024] Embodiment 1,

[0025] A method for wet recovery of nickel-cobalt-lithium manganese oxide waste comprises the following steps:

[0026] A. 3000 g of lithium nickel cobalt manganate waste was calcined at 600° C. under air flow for 2 h to obtain a calcined material;

[0027] B. Take 1000g of the calcined material obtained in step A, add 250ml of concentrated sulfuric acid, 350ml of hydrogen peroxide and 2700ml of pure water, raise the temperature to 95°C, react for 80min, separate the solid and liquid to obtain leached residue I and leached solution I, the temperature of leached solution I is 64°C, the concentration of manganese in leached solution I is 90g / L, and the total concentration of nickel and cobalt is 210g / L; return the leached residue I to step B for further leaching and dissolving;

[0028] C. The leachate I obtained in step B is heated to 68° C., and then calcined materials, hydrogen peroxide and concentrated sulfuric acid are added, the reaction temperature is 90° C., the reaction time is 2 h, and the temperature of the filtered liquid is maintained at 64° C. to obtain leachate II and leach residue II, wherein the concentration of manganese in leachate II is 180 g / L, and the total concentration of cobalt and nickel is 420 g / L; the leachate II is heated to 98° C., solid-liquid separation is performed while hot, and the temperature of the filtered liquid is maintained at 95° C. to obtain manganese sulfate crystals and leachate III, and the temperature of the leachate III is further reduced to 27° C. to obtain mixed crystals of cobalt sulfate and nickel sulfate and leachate IV; the leach residue II is returned to step B for further leaching and dissolution;

[0029] D. Raising the temperature of leachate IV to 68° C., adding calcined material, hydrogen peroxide and concentrated sulfuric acid, and continuously repeating the operation of step C to continuously precipitate manganese sulfate crystals and mixed crystals of cobalt sulfate and nickel sulfate; in the repeated process, when the lithium content in the leachate is enriched to 20 g / L, stopping the feeding, raising the temperature of the leachate to not less than 90° C., adding sodium hydroxide to adjust the pH to 12, and filtering by sedimentation to obtain a mixture of cobalt hydroxide, nickel hydroxide and manganese hydroxide, and a lithium sulfate solution;

[0030] E. Add sodium carbonate to the lithium sulfate solution obtained in step D to react, wherein the amount of sodium carbonate used is 9 times the total lithium mass in the lithium sulfate solution, the reaction time is 60 min, the reaction temperature is 90° C., and solid-liquid separation is performed to obtain lithium carbonate and carbonized liquid;

[0031] F. After carbonization, sulfuric acid is added to the liquid to adjust the pH to 5, and then the liquid is frozen at a temperature of -10°C for 60 minutes, and solid-liquid separation is performed to obtain sodium sulfate decahydrate and a lithium sulfate solution without sodium sulfate;

[0032] The obtained lithium sulfate solution without sodium sulfate is returned to step B for further leaching;

[0033] The obtained sodium sulfate decahydrate is subjected to hot melting treatment, and the volume is evaporated and concentrated to 1 / 2 of the original volume, and the solid-liquid separation is performed while hot to obtain a lithium-containing solution and sodium sulfate;

[0034] The obtained lithium-containing solution was added with 1.05 times the theoretical amount of phosphoric acid, and sodium hydroxide was added to adjust the pH to 10. The reaction temperature was 90° C. and the reaction time was 50 min. Lithium phosphate was obtained by solid-liquid separation.

[0035] Embodiment 2-4,

[0036] The difference between Example 2-4 and Example 1 is that the calcination temperature is different in step A. The effect of calcination temperature on the comprehensive recovery rate of nickel, cobalt, manganese and lithium is shown in Table 1.

[0037]

[0038] As shown in Table 1, when the calcination temperature is between 600 and 700°C, the comprehensive recovery rate of nickel, cobalt, manganese and lithium is relatively high, and further increasing the temperature has little effect on the recovery rate of lithium. Therefore, the calcination temperature is preferably selected to be 600°C.

[0039] Embodiment 6-11,

[0040] The difference between Examples 6-11 and Example 1 is that in step B, the concentrations of nickel, cobalt and manganese in the leaching solution I are different. The influence of different concentrations of nickel, cobalt and manganese in the leaching solution I on the precipitation of manganese sulfate and mixed crystals of cobalt sulfate and nickel sulfate is shown in Table 2.

[0041]

[0042] As shown in Table 2, when the concentration of manganese is 50-95 g / L, and the concentration of nickel and cobalt is 100-200 g / L, no manganese sulfate, nickel sulfate and cobalt sulfate crystals will be precipitated. Therefore, the concentration of manganese leaching is preferably controlled at 85-90 g / L, and the concentration of nickel and cobalt is controlled at 200-210 g / L.

[0043] Embodiment 12-22,

[0044] The difference between Examples 12-22 and Example 1 is that in step C, the concentrations of nickel, cobalt and manganese in the leaching solution II are different. The influence of different concentrations of nickel, cobalt and manganese in the leaching solution II on the precipitation of manganese sulfate crystals and mixed crystals of cobalt sulfate and nickel sulfate is shown in Table 3.

[0045]

[0046] As shown in Table 3, when the manganese concentration is 120-180 g / L, and the nickel and cobalt concentrations are 240-420 g / L, manganese sulfate crystals and mixed crystals of nickel sulfate and cobalt sulfate will not be precipitated. Therefore, the manganese concentration of the leaching solution is preferably controlled at 180-190 g / L, and the nickel and cobalt concentrations are controlled at 400-420 g / L.

[0047] Embodiment 23-29,

[0048] The difference between Examples 23-29 and Example 1 is that in step C, after solid-liquid separation, the temperature of the filtered liquid is different. The effect of the filtered liquid temperature on whether manganese sulfate crystals can be obtained is shown in Table 4.

[0049]

[0050] As shown in Table 4, manganese sulfate crystals will precipitate when the temperature of the filtered liquid is 80-95°C. Therefore, the filtered liquid temperature is preferably 90-95°C. The higher the filtered liquid temperature, the more manganese sulfate crystals are precipitated. The solubility of manganese sulfate is negatively correlated with temperature.

[0051] Embodiment 30-37,

[0052] The difference between Examples 30-37 and Example 1 is that in step C, when the leaching solution III is reduced to different temperatures, the influence of reducing the leaching solution III to different temperatures on whether mixed crystals of nickel sulfate and cobalt sulfate can be obtained is shown in Table 5.

[0053]

[0054] As shown in Table 5, nickel sulfate and cobalt sulfate crystals will precipitate when the temperature of the filtered liquid is 25-50°C. Therefore, the cooling temperature is preferably 25-30°C. The lower the cooling temperature, the more nickel sulfate and cobalt sulfate crystals are precipitated. The solubility of nickel sulfate and cobalt sulfate is positively correlated with temperature.

[0055] Embodiment 38-47,

[0056] The difference between Examples 38-47 and Example 1 is that the lithium enrichment concentration is different in step D. The influence of different lithium enrichment concentrations on whether lithium sulfate is precipitated at room temperature is shown in Table 6.

[0057]

[0058] It can be seen from Table 6 that lithium sulfate crystals will not precipitate when the concentration of lithium enrichment is 10-25 g / L. Therefore, the concentration of lithium enrichment is preferably 20-25 g / L.

[0059] Embodiment 48-52,

[0060] The difference between Examples 48-52 and Example 1 is that the reaction time is different in step E. The effect of reaction time on the conversion rate of lithium carbonate is shown in Table 7.

[0061]

[0062] It can be seen from Table 7 that when the reaction time is 40-60 min, the conversion rate of lithium carbonate is higher. Therefore, the optimal reaction time is 40 min.

[0063] Embodiment 53-57,

[0064] The difference between Examples 53-57 and Example 1 is that different amounts of sodium carbonate are used in step E. The effect of reaction time on the conversion rate of lithium carbonate is shown in Table 8.

[0065]

[0066] As shown in Table 8, when the amount of sodium carbonate is 9-10 times of the total mass, the conversion rate of lithium carbonate is higher. Therefore, the amount of sodium carbonate is preferably selected to be 9 times of the total mass.

[0067] Embodiment 58-67,

[0068] The difference between Examples 58-67 and Example 1 is that the freezing is different in step F. The effect of freezing temperature on the sodium ion content in the solution is shown in Table 9.

[0069]

[0070] It can be seen from Table 9 that when the freezing temperature is between -8 and -10°C, the sodium ion content is low. Therefore, the optimal freezing temperature is -10°C.

[0071] Embodiment 68-74,

[0072] The difference between Examples 68-74 and Example 1 is that in step F, sodium hydroxide is added to adjust the pH to different pH values. The effect of different pH values ​​on the recovery rate of lithium phosphate obtained is shown in Table 10.

[0073]

[0074] It can be seen from Table 10 that when the pH value is 10-12, the recovery of lithium phosphate is higher. Therefore, the pH value is preferably selected to be 10-11.

[0075] Embodiment 75-79,

[0076] The difference between Examples 75-79 and Example 1 is that the reaction time is different in step F. The effect of reaction time on the recovery rate of lithium phosphate is shown in Table 11.

[0077]

[0078] It can be seen from Table 11 that when the reaction time is 40-60 min, the recovery of lithium phosphate is higher. Therefore, the reaction time is preferably selected to be 40 min.

[0079] Embodiment 80-84,

[0080] The difference between Examples 80-84 and Example 1 is that different amounts of phosphoric acid are used in step F. The effect of the amount of phosphoric acid on the recovery rate of lithium phosphate is shown in Table 12.

[0081]

[0082] It can be seen from Table 11 that when the amount of phosphoric acid is 1.04-1.05 times, the recovery of lithium phosphate is higher. Therefore, the amount of phosphoric acid is preferably selected to be 1.05 times the theoretical amount.

[0083] Comparative Example 1

[0084] This comparative example uses a traditional ternary recovery process, which roughly uses sulfuric acid and hydrogen peroxide as leaching solvents to dissolve the valuable metals nickel, cobalt, manganese and lithium in nickel, cobalt and manganese oxide to generate a leachate of nickel sulfate, cobalt sulfate, manganese sulfate and lithium sulfate, and then add a large amount of sodium hydroxide to adjust the pH to 12 to obtain nickel, cobalt and manganese hydroxide and lithium sulfate solution. In the process of adding sodium hydroxide, a large amount of nickel sulfate, cobalt sulfate and manganese sulfate are converted into a mixed precipitate of nickel hydroxide, cobalt hydroxide and manganese hydroxide, accompanied by a large amount of sodium sulfate decahydrate. The obtained lithium sulfate solution continues to add sodium carbonate to precipitate and obtain lithium carbonate, achieving the purpose of recovering lithium, and is also accompanied by the production of sodium sulfate decahydrate. The above two valuable metal recovery are accompanied by the generation of a large amount of sodium sulfate decahydrate. The crystal water in the sodium sulfate decahydrate will take away more valuable metal lithium after solid-liquid separation, causing lithium loss.

[0085] Five parallel experiments were conducted in this comparative example, and the lithium recovery rates obtained were 90%, 89%, 89%, 88% and 90%, respectively.

[0086] In addition, five parallel experiments were conducted in Example 1, and the lithium recovery rates obtained were 97.2%, 97.1%, 97.1%, 97.3% and 97.1%, respectively.

[0087] It can be seen that the traditional process for recovering valuable metal lithium from waste nickel-cobalt-manganese-oxide lithium waste has a lithium recovery rate of about 90%. The lithium recovery rate of the method of the present invention is about 97%, which is much higher than the traditional method, and the process is simple and easy to mass produce.

Claims

1. A method for wet recovery of nickel-cobalt-manganese-lithium oxide waste, characterized in that The following steps are involved: A. calcining nickel-cobalt-lithium manganate waste under air flow to obtain a calcined material; B. Add concentrated sulfuric acid, hydrogen peroxide and pure water to the calcined material obtained in step A, raise the temperature to 80-90° C., react for 1-3 hours, separate the solid and liquid to obtain leached residue I and leached solution I, wherein the concentration of manganese in the leached solution I is 85-90 g / L, and the total concentration of nickel and cobalt is 200-210 g / L. After filtering, the temperature of the leached solution I is maintained at 60-70° C.; C. The leachate I obtained in step B is heated to 65-70° C., and then the calcined material, hydrogen peroxide and concentrated sulfuric acid are added, the reaction time is 1-3h, and the temperature of the filtered liquid is maintained at 60-65° C. to obtain leachate II and leach residue II, wherein the concentration of manganese in the leachate II is 170-180g / L, and the total concentration of cobalt and nickel is 400-420g / L; the leachate II is heated to not less than 95° C., solid-liquid separation is performed while hot, and the temperature of the filtered liquid is maintained at 90-95° C. to obtain manganese sulfate crystals and leachate III, and the temperature of the leachate III is further reduced to 25-30° C. to obtain mixed crystals of cobalt sulfate and nickel sulfate and leachate IV; D. Raise the temperature of the leachate IV to 65-70° C., add the calcined material, hydrogen peroxide and concentrated sulfuric acid, repeat the operation of step C, and repeat the operation continuously to continuously precipitate manganese sulfate crystals and mixed crystals of cobalt sulfate and nickel sulfate; during the repetitive process, when the lithium content in the leachate is enriched to 20-25 g / L, stop adding the material, raise the temperature of the leachate to not less than 90° C., add sodium hydroxide to adjust the pH to 11-12, and separate the solid and liquid to obtain a ternary precursor and a lithium sulfate solution; E. Adding sodium carbonate to the lithium sulfate solution obtained in step D to react, and separating the solid and liquid to obtain lithium carbonate and carbonized liquid; F. After carbonization, sulfuric acid is added to the liquid to adjust the pH to 5-6, and then the liquid is frozen at a temperature of -10-0°C for 30-60 minutes. The solid-liquid separation is performed to obtain sodium sulfate decahydrate and a lithium sulfate solution free of sodium sulfate.

2. The method for wet recovery of nickel-cobalt-lithium manganese oxide waste according to claim 1, characterized in that: In step A, the calcination temperature is 600-700° C., and the calcination time is 1-3 hours.

3. A method for wet recovery of nickel-cobalt-lithium manganese oxide waste according to claim 1 or 2, characterized in that: In step E, the reaction time is 40-60 min, and the reaction temperature is 90-100°C.

4. The method for wet recovery of nickel-cobalt-lithium manganese oxide waste according to claim 3, characterized in that: In step E, the amount of sodium carbonate used is 9-9.5 times the total mass of lithium in the lithium sulfate solution.

5. The method for wet recovery of nickel-cobalt-lithium manganese oxide waste according to claim 4, characterized in that: In step F, the obtained lithium sulfate solution free of sodium sulfate is returned to step B for further leaching.

6. The method for wet recovery of nickel-cobalt-lithium manganese oxide waste according to claim 4, characterized in that: In step F, the obtained sodium sulfate decahydrate is subjected to heat melting treatment, and the volume is evaporated and concentrated to 1 / 3-1 / 2 of the original volume, and the solid-liquid separation is performed while hot to obtain a lithium-containing solution and sodium sulfate.

7. The method for wet recovery of nickel-cobalt-lithium manganese oxide waste according to claim 6, characterized in that: In step F, phosphoric acid is added to the obtained lithium-containing solution, and sodium hydroxide is added to adjust the pH to 10-11 to prepare lithium phosphate.

8. The method for wet recovery of nickel-cobalt-lithium manganese oxide waste according to claim 7, characterized in that: In step F, when preparing lithium phosphate, the reaction temperature is not less than 90° C. and the reaction time is 40-60 min.

9. The method for wet recovery of nickel-cobalt-lithium manganese oxide waste according to claim 8, characterized in that: In step F, when preparing lithium phosphate, the amount of phosphoric acid used is 1.04-1.05 times the theoretical amount.

Citation Information

Patent Citations

  • Method for recycling valuable metal in manganese-rich slag

    CN102242267A

  • Method for recycling lithium, nickel, cobalt and manganese from waste ternary anode material

    CN107666022A

  • A method for recovering valuable metals from waste lithium ion batteries

    CN108963371A

  • Lithium battery waste recycling method and application thereof

    CN113106257A

  • Recovery method of metals from recycled raw material of lithium-ion battery

    JP2016186118A