A super-high concentration cationic emulsion polymer flocculant and preparation method thereof
By using homemade amphiphilic polymer stabilizers and composite initiators in reverse phase emulsions, a high-concentration cationic emulsion flocculant was prepared, which solved the problems of difficulty in dissolution and low concentration of traditional products, and achieved efficient and stable cationic polymer flocculation. Agent, suitable for offshore oil fields and industrial water treatment.
Patent Information
- Application Number
- CN202310462368.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-26
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-04-26
AI Technical Summary
Traditional cationic polyacrylamide powder products have problems such as laborious, slow dissolution speed, harsh environment and high transportation costs during the dissolution process. The concentration of conventional reverse phase emulsion polymers is low, which cannot meet the high concentration needs of users, especially at sea. There are difficulties in the application of oil field platforms.
Using the preparation method of ultra-high concentration cationic emulsion polymer flocculant, the polymerization is gradually improved by adding homemade amphiphilic polymer stabilizer, composite surfactant and composite initiator to the reverse phase emulsion. The concentration and molecular weight of the substance can achieve high concentration and stability.
Prepare ultra-high concentration cationic emulsion polymer flocculant with a concentration of ≥65%, which has good low temperature resistance, instant solubility and storage stability, significantly saves transportation costs, and is suitable for offshore oil fields and industrial water treatment.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of preparation of high molecular polymers, and in particular relates to an ultra-high concentration cationic emulsion polymer flocculant and a preparation method thereof. Background Art
[0002] Cationic polyacrylamide (CPAM) is a linear polymer compound. Because it has a variety of active groups, it can form hydrogen bonds with many substances by adsorption, can flocculate negatively charged colloids, and has the functions of decolorization, adsorption, bonding, and turbidity removal. It is widely used in wastewater treatment with high organic impurity content in industries such as papermaking, dyeing and finishing, mineral processing, oil fields, food, and brewing. It is particularly suitable for the dehydration of urban sludge, papermaking sludge and other industrial sludge. Due to its wide range of uses, it is the most important synthetic water-soluble polymer. There are many problems in the use of traditional powder products of cationic polyacrylamide: laborious dissolution, poor working environment, slow dissolution speed, and large dissolution equipment. The domestic and foreign markets have gradually shifted from powder products to emulsion products, but the conventional PAM latex products obtained by inverse emulsion polymerization have low concentrations (25% to 35%), high transportation costs, and poor storage stability, which cannot meet user needs well. Ultra-high concentration cationic polyacrylamide emulsion can significantly save transportation costs. It can be widely used in areas such as offshore oilfield platforms where the working space is relatively narrow. Based on this, this technology can prepare ultra-high concentration cationic polymer flocculants, which can replace cationic polymer dry powder on a large scale and have broad prospects. Summary of the invention
[0003] In view of this, the present invention aims to provide an ultra-high concentration cationic emulsion polymer flocculant and a preparation method thereof. The prepared ultra-high concentration cationic emulsion polymer flocculant has the characteristics of ultra-high concentration, high molecular weight, good low temperature resistance, rapid solubility and storage stability.
[0004] To achieve the above object, the technical solution of the present invention is implemented as follows: a method for preparing an ultra-high concentration cationic emulsion polymer flocculant comprises the following steps:
[0005] Step 1, adding an organic solvent, a composite surfactant, a homemade amphiphilic polymer stabilizer and an oil-soluble initiator into an oil phase batching tank, stirring and dissolving them fully;
[0006] Step 2, adding acrylamide monomer, cationic monomer, complexing agent, composite water-soluble initiator system and deionized water into a water phase tank and stirring to fully dissolve;
[0007] Step 3, slowly pump the material in the water phase tank into the oil phase tank, stir the material in the oil phase tank during the pumping process, and then use an emulsifier to emulsify the material in the oil phase tank for 15 minutes. After the particle size is tested to be qualified, the emulsified emulsion is pumped into the reactor, stirring is started, and nitrogen is filled for more than 1 hour;
[0008] Step 4: Use cooling brine to lower the temperature of the reactor to 15°C and continue to charge with nitrogen;
[0009] Step 5: Prepare the reducing agent solution, add oil and emulsifier, and emulsify with an emulsifier for standby use; slowly drop the reducing agent solution into the reactor with a metering pump, and adjust the reducing agent dropping speed according to the temperature rise;
[0010] Step 6, when the temperature of the reactor reaches 40°C, add the initiator dropwise at a constant temperature until the configured initiator is completely added to the reactor, raise the temperature of the reactor step by step to 50°C, 60°C and 70°C, react for one hour respectively, and then stop nitrogen filling;
[0011] Step 7, the emulsion after the reaction is completed is poured into a distillation reactor, and the temperature is maintained at 70°C-80°C and the vacuum distillation is performed until the effective concentration is ≥ 66.5%;
[0012] Step 8: Add 1%-1.5% of a phase inversion agent to the distillation reaction to invert the phase, and obtain a super-high concentration cationic emulsion polymer product with a concentration of ≥65%.
[0013] Furthermore, the organic solvent is white oil and D60 solvent oil in a ratio of 1:3;
[0014] The composite surfactant is any two of span85, span80, and span60, with a weight ratio of 1:1, and after mixing, is compounded with any one of Tween80 and Tween81, with a compound weight ratio of 1:1.
[0015] Further, the homemade amphiphilic polymer stabilizer is a copolymer of any two monomers of tetradecyl acrylate, hexadecyl acrylate, octadecyl acrylate and docosyl acrylate, the monomer compounding ratio is 1:1, and the viscosity of the 40% solution of the amphiphilic polymer stabilizer is required to be 300-800cp;
[0016] The oil-soluble initiator is a compound of azobisisobutyronitrile and azobisisovaleronitrile, and the weight ratio is 1:2.
[0017] Further, the cationic monomer is one or both of acryloyloxyethyl trimethyl ammonium chloride and methacrylamide ethyl trimethyl ammonium chloride;
[0018] The complexing agent is one or more of sodium ethylenediaminetetraacetate, sodium ethylenediaminetetrapropionate, and sodium diethylenetriaminepentaacetate.
[0019] Furthermore, the composite water-soluble initiator system is ammonium persulfate, azobisisobutylimidazoline hydrochloride and azobisisobutylamidine hydrochloride, and the ratio of the three initiators is 3:1:1.
[0020] Furthermore, the reducing agent concentration is 1.5%-2%; the reducing agent is one or more of sodium bisulfite, sodium sulfite and sodium pyrosulfite.
[0021] Furthermore, the phase transfer agent is any two of nonylphenol polyoxyethylene ether, octylphenol polyoxyethylene ether and polyoxyethylene ether natural fatty alcohol, with a ratio of 1:1.
[0022] Furthermore, the polymer raw material, by weight, includes the following components:
[0023] 280-290 parts of organic solvent, 2-3 parts of composite surfactant, 1-2 parts of homemade amphiphilic polymer stabilizer, 0.05-0.1 parts of oil-soluble initiator, 210-240 parts of acrylamide monomer, 140-160 parts of cationic monomer, 0.05-0.08 parts of complexing agent, 0.07-0.08 parts of composite water-soluble initiator system and 0.05-0.06 parts of reducing agent.
[0024] An ultra-high concentration cationic emulsion polymer flocculant is prepared by any of the above-mentioned methods for preparing an ultra-high concentration cationic emulsion polymer flocculant, and its concentration is ≥65%.
[0025] Furthermore, the molecular weight of the emulsion polymer flocculant is greater than 8 million.
[0026] Compared with the prior art, the ultra-high concentration cationic emulsion polymer flocculant and the preparation method thereof described in the present invention have the following advantages:
[0027] (1) The present invention can prepare an ultra-high concentration cationic emulsion polymer with an effective concentration of ≥65% by adding an amphiphilic polymer stabilizer prepared with different block lengths in the oil phase prepared by the inverse emulsion. At the same time, the block length of the amphiphilic polymer stabilizer can be adjusted to prepare an ultra-high concentration cationic polymer emulsion with excellent low temperature resistance;
[0028] (2) The present invention can prepare ultra-high concentration cationic polymer emulsions with different HLB values by adjusting the type and amount of the composite surfactant. When the amount of the phase inversion agent is the same, ultra-high concentration cationic polymer emulsion products with different dissolution rates can be obtained to meet the needs of different occasions;
[0029] (3) The present invention adopts a composite oil-soluble initiator. The two oil-soluble initiators have different decomposition temperatures. Therefore, they can continue to decompose and initiate at 60-80° C., and the ultra-high concentration cationic polymer emulsion product has lower residual monomers, which better meets environmental protection requirements;
[0030] (4) The present invention adopts a composite water-soluble initiator system. During the initial and middle stages of the reaction, different initiators decompose at different temperatures, and polymerization is initiated step by step, thereby facilitating the preparation of a high molecular weight emulsion polymer product.
[0031] (5) The present invention can control the reaction speed by controlling the speed of dripping the reducing agent, can adjust the slow release of reaction heat, and can obtain an ultra-high concentration cationic polymer emulsion product with higher molecular weight and better solubility;
[0032] (6) The present invention can complex metal ions by adding a complexing agent, thereby increasing the activity of the polymerization monomer and further increasing the molecular weight of the ultra-high concentration cationic emulsion polymer product.
[0033] In summary, the ultra-high concentration cationic emulsion polymer flocculant prepared by the present invention has the following characteristics: ultra-high concentration, high molecular weight, good low temperature resistance, rapid solubility and storage stability. DETAILED DESCRIPTION
[0034] In the following description, a large number of specific details are provided to provide a more thorough understanding of the present invention. However, it is apparent to those skilled in the art that the present invention can be implemented without one or more of these details. In other examples, in order to avoid confusion with the present invention, some technical features well known in the art are not described.
[0035] The invention discloses an ultra-high concentration cationic emulsion polymer flocculant and a preparation method thereof, which adopts reverse emulsion polymerization, a composite emulsification system, and a low-temperature composite initiation system for segmented initiation, and adds a homemade amphiphilic polymer stabilizer in the oil phase, the stabilizer can ensure that the emulsion is concentrated to an ultra-high concentration and remains stable, and an ultra-high concentration cationic polymer emulsion with an effective concentration of ≥65% is prepared. The core technology of the invention is to prepare an amphiphilic polymer stabilizer with a special structure. Under the action of this type of amphiphilic polymer stabilizer, an ultra-high concentration cationic emulsion polymer with excellent stability can be prepared, and then assisted by low-temperature composite initiation technology, a high molecular weight ultra-high concentration cationic emulsion polymer product can be prepared, which has broad application prospects in industrial water treatment and offshore oil field oil-water separation.
[0036] The present invention provides a method for preparing an ultra-high concentration cationic emulsion polymer flocculant, comprising the following steps:
[0037] Step 1, adding an organic solvent, a composite surfactant, a homemade amphiphilic polymer stabilizer and an oil-soluble initiator into an oil phase batching tank, stirring and dissolving them fully;
[0038] Step 2, adding acrylamide monomer, cationic monomer, complexing agent, composite water-soluble initiator system and deionized water into a water phase tank and stirring to fully dissolve;
[0039] Wherein, the cationic monomer is one or both of acryloyloxyethyl trimethyl ammonium chloride and methyl acrylamide ethyl trimethyl ammonium chloride; the complexing agent is one or more of sodium ethylenediaminetetraacetate, sodium ethylenediaminetetrapropionate, and sodium diethylenetriaminepentaacetate.
[0040] Step 3, slowly pump the material in the water phase tank into the oil phase tank, stir the material in the oil phase tank during the pumping process, and then use an emulsifier to emulsify the material in the oil phase tank for 15 minutes. After the particle size is tested to be qualified, the emulsified emulsion is pumped into the reactor, stirring is started, and nitrogen is filled for more than 1 hour;
[0041] Step 4: Use cooling brine to lower the temperature of the reactor to 15°C and continue to charge with nitrogen;
[0042] Step 5, prepare a reducing agent solution with a concentration of 1.5%-2%, add oil and emulsifier and emulsify it with an emulsifier for standby use, slowly drop the reducing agent solution into the reactor with a metering pump, and adjust the reducing agent dropping speed according to the temperature rise; the reducing agent is one or more of sodium bisulfite, sodium sulfite and sodium pyrosulfite.
[0043] Step 6, when the temperature of the reactor reaches 40°C, add the initiator dropwise at a constant temperature until the configured initiator is completely added to the reactor, raise the temperature of the reactor step by step to 50°C, 60°C and 70°C, react for one hour respectively, and then stop nitrogen filling;
[0044] Step 7, the emulsion after the reaction is completed is poured into a distillation reactor, and the temperature is maintained at 70°C-80°C and the vacuum distillation is performed until the effective concentration is ≥ 66.5%;
[0045] Step 8: Add 1%-1.5% of a phase inversion agent to the distillation reaction to invert the phase, and obtain a super-high concentration cationic emulsion polymer product with a concentration of ≥65%.
[0046] The self-made amphiphilic polymer stabilizer is a copolymer of any two monomers of tetradecyl acrylate, hexadecyl acrylate, octadecyl acrylate and docosyl acrylate, the monomer compounding ratio is 1:1, and the viscosity of a 40% solution of the amphiphilic polymer stabilizer is required to be 300-800cp.
[0047] The invention can maintain the emulsion in a stable state by adding a self-made amphiphilic polymer stabilizer to the emulsion oil phase during high-temperature distillation to an effective concentration of about 65%. After the amphiphilic polymer stabilizer is added to the emulsion system, in addition to the emulsifier stabilization layer, an amphiphilic polymer stabilizer stabilization layer is added to the outer layer of the latex particles. During concentration, as the light oil in the emulsion system is distilled out, the distance between the latex particles becomes closer and closer, and the collision and friction of the latex particles become more and more. If the amphiphilic polymer stabilizer is not added, the latex particles are very close to each other and are prone to aggregation, which may cause demulsification in severe cases. After the amphiphilic polymer stabilizer is added to the emulsion system, the outer layer of the latex particles has an amphiphilic polymer stabilizer protective layer, which reduces the interfacial tension of the particles. Even if the collision of the latex particles intensifies, the latex particles can be kept intact, thereby achieving the purpose of maintaining the stability of the emulsion during the concentration process and after the concentration. In addition, the length of the chain segment of the amphiphilic polymer stabilizer has a great influence on the low temperature resistance of the emulsion. When different stabilizers are added, a protective layer of amphiphilic polymer stabilizer is formed on the outermost layer of the latex particles, which reduces the friction resistance between the particles like an elastomer, improves the flow performance of the emulsion, and thus improves the low temperature resistance of the emulsion. As the long-chain monomers in the structural units of the emulsion added with amphiphilic polymer stabilizers change from long to short, the low temperature resistance of the emulsion system also changes from weak to strong. The reason may be that the longer the chain of the amphiphilic polymer stabilizer structural unit, the worse the temperature resistance of the emulsion after adding it. This is probably mainly determined by the freezing point of the structural unit in the stabilizer itself, that is, the lower the freezing point of the amphiphilic polymer stabilizer structural unit, the better the low temperature resistance of the emulsion.
[0048] In a further embodiment, the organic solvent is white oil and D60 solvent oil in a ratio of 1:3.
[0049] The invention adds white oil and D60 to the emulsion at a compounding ratio of 1:3. The reason for adding two kinds of oils with a relatively large difference in boiling points is that when the concentration is just started and the vacuum degree and temperature are relatively low, low-boiling-point oil and water are first distilled out, and as the vacuum pressure increases and the temperature rises, a part of high-boiling-point oil is also distilled out later. The purpose of such compounding is mainly to allow the emulsion polymer to slowly distill out the oil and water in stages, so that the emulsion is always concentrated in a relatively mild environment until the concentration is concentrated to more than 65%.
[0050] In a further embodiment, the composite surfactant is any two of span85, span80, and span60, which are mixed in a weight ratio of 1:1 and then compounded with any one of Tween80 and Tween81, and the compound weight ratio is 1:1.
[0051] First, the present invention adopts a Span series and a Tween series emulsifier to form a composite emulsification system; by selecting an emulsifier with an HLB value lower than 6 and another emulsifier with an HLB value higher than 10 for composite, an emulsion system with an HLB value of any value between 6 and 8 can be obtained, thereby obtaining an ultra-high concentration emulsion polymer with different dissolution rates, thereby meeting different environmental requirements.
[0052] In a further embodiment, the composite water-soluble initiator system is ammonium persulfate, azobisisobutylimidazoline hydrochloride and azobisisobutylamidine hydrochloride, and the ratio of the three initiators is 3:1:1. The oil-soluble initiator is a compound of azobisisobutyronitrile and azobisisovaleronitrile, and the weight compound ratio is 1:2.
[0053] Since the thermal initiators have different decomposition temperatures, when multiple thermal initiators are used in combination, they can decompose at different temperatures, and can achieve step-by-step polymerization, thereby increasing the molecular weight of the polymer, while reducing the excessive branching structure caused by the concentrated decomposition of one initiator and reducing the solubility of the product. Similarly, the present invention simultaneously uses two oil-soluble initiators with different decomposition temperatures, which can complement the water-soluble composite initiation system, gradually initiate polymerization in sections, thereby increasing the molecular weight of the polymer and reducing the residual monomer content.
[0054] In a further embodiment, the phase transfer agent is any two of nonylphenol polyoxyethylene ether, octylphenol polyoxyethylene ether and polyoxyethylene ether natural fatty alcohol, and the ratio is 1:1.
[0055] The reason why the inverse emulsion needs phase inversion is that before the phase inversion, the surface of the latex particles is well wrapped by the emulsifier, and the product cannot be quickly dissolved in water. After adding the phase inversion agent, hydrophilic channels are left on the surface of the latex particles. Once dispersed in water, water can quickly enter the latex particles from the hydrophilic channels, thereby achieving the purpose of rapid dissolution. Adding two emulsifiers with HLB greater than 10 as a phase inversion agent, the strength of the hydrophilic channels formed on the surface of the latex particles varies to a certain extent, which can adjust the speed at which water enters the latex particles during dissolution, thereby adjusting the solubility performance of the ultra-high concentration cationic polymer emulsion.
[0056] The polymer raw material, calculated by weight, includes the following components:
[0057] 280-290 parts of organic solvent, 2-3 parts of composite surfactant, 1-2 parts of homemade amphiphilic polymer stabilizer, 0.05-0.1 parts of oil-soluble initiator, 210-240 parts of acrylamide monomer, 140-160 parts of cationic monomer, 0.05-0.08 parts of complexing agent, 0.07-0.08 parts of composite water-soluble initiator system and 0.05-0.06 parts of reducing agent.
[0058] An ultra-high concentration cationic emulsion polymer flocculant is prepared by any of the above-mentioned methods for preparing an ultra-high concentration cationic emulsion polymer flocculant, wherein the concentration of the ultra-high concentration cationic emulsion polymer flocculant is ≥65%, and the molecular weight of the emulsion polymer flocculant is higher than 8 million. The ultra-high concentration cationic emulsion polymer flocculant can be used as a flocculant to treat industrial wastewater, and can also be used as a sludge dewatering agent.
[0059] The present invention will be further described below in conjunction with embodiments. The examples of the embodiments are intended to explain the present invention and should not be construed as limiting the present invention.
[0060] Example 1
[0061] 280 parts of organic solvent, 2 parts of composite surfactant, 1 part of self-made amphiphilic polymer stabilizer, 0.06 parts of oil-soluble initiator are added to the oil phase batching tank and stirred thoroughly to dissolve; 210 parts of acrylamide monomer, 160 parts of cationic monomer, 0.06 parts of complexing agent, 0.07 parts of composite water-soluble initiator system and deionized water are added to the water phase tank and stirred thoroughly to dissolve; the materials in the water phase tank are slowly pumped into the oil phase tank while stirring, and emulsified for 15 minutes with an emulsifier, and after the particle size is tested to be qualified, the emulsified emulsion is pumped into the reactor, stirring is started, and nitrogen is filled for more than 1 hour; the temperature of the reactor is reduced to 15°C with cooling brine, and nitrogen is continued to be filled; a solution with a reducing agent concentration of 1.6% is prepared, and oil and emulsifier are added and emulsified with an emulsifier for standby use, and the reducing agent emulsion is slowly dripped into the reactor with a metering pump, and the reducing agent dripping speed is adjusted according to the temperature rise. When the temperature of the reactor reaches 40°C, the reducing agent is added dropwise at a constant temperature until the configured reducing agent is completely added to the reactor. The total amount of reducing agent added is 0.05 parts. The temperature of the reactor is gradually raised to 50°C, 60°C and 70°C for one hour each, and nitrogen filling is stopped. The emulsion that has reacted completely is poured into the distillation reactor, and the temperature is maintained at 70°C-80°C and distilled under reduced pressure to a concentration of 66.5%. 1% of a phase inversion agent is added to the distillation reaction to invert the phase, and a super-high concentration cationic emulsion polymer product with a molecular weight of 9.2 million, a bulk viscosity of 1680cp and a concentration of 65.8% is obtained.
[0062] Example 2
[0063] 280 parts of organic solvent, 2 parts of composite surfactant, 1.5 parts of self-made amphiphilic polymer stabilizer and 0.07 parts of oil-soluble initiator are added to the oil phase batching tank and stirred to dissolve; 230 parts of acrylamide monomer, 150 parts of cationic monomer, 0.06 parts of complexing agent, 0.07 parts of composite water-soluble initiator system and deionized water are added to the water phase tank and stirred to dissolve; the materials in the water phase tank are slowly pumped into the oil phase tank while stirring, and emulsified for 15 minutes with an emulsifier, and after the particle size is tested to be qualified, the emulsified emulsion is pumped into the reactor, stirring is started, and nitrogen is filled for more than 1 hour; the temperature of the reactor is reduced to 15°C with cooling brine, and nitrogen is continued to be filled; a solution with a reducing agent concentration of 2% is prepared, and oil and emulsifier are added and emulsified with an emulsifier for standby use, and the reducing agent is slowly added dropwise to the reactor with a metering pump, and the reducing agent dropping speed is adjusted according to the temperature rise. When the temperature of the reactor reaches 40°C, the initiator is added dropwise at a constant temperature until the prepared reducing agent is completely added to the reactor. The total amount of reducing agent added is 0.05 parts. The temperature of the reactor is gradually raised to 50°C, 60°C and 70°C for one hour each, and nitrogen filling is stopped. The emulsion that has reacted completely is poured into the distillation reactor, and the temperature is maintained at 70°C-80°C and distilled under reduced pressure to a concentration of 67.5%. 1.2% of the phase inversion agent is added to the distillation reaction to invert the phase, and a super-high concentration cationic emulsion polymer product with a molecular weight of 10.2 million, a bulk viscosity of 1735cp and a concentration of 66.7% is obtained.
[0064] Example 3
[0065] 290 parts of organic solvent, 2.5 parts of composite surfactant, 2 parts of self-made amphiphilic polymer stabilizer and 0.08 parts of oil-soluble initiator are added to the oil phase batching tank and stirred to dissolve; 240 parts of acrylamide monomer, 140 parts of cationic monomer, 0.08 parts of complexing agent, 0.07 parts of composite water-soluble initiator system and deionized water are added to the water phase tank and stirred to dissolve; the materials in the water phase tank are slowly pumped into the oil phase tank while stirring, and emulsified for 15 minutes with an emulsifier. After the particle size is tested to be qualified, the emulsified emulsion is pumped into the reactor, stirred and filled with nitrogen for more than 1 hour; the temperature of the reactor is reduced to 15°C with cooling brine, and nitrogen is continued to be filled; a solution with a reducing agent concentration of 2% is prepared, and oil and emulsifier are added for emulsification for standby use, and the reducing agent is slowly added dropwise to the reactor with a metering pump, and the dropping speed of the reducing agent is adjusted according to the temperature rise. When the temperature of the reactor reaches 40°C, the reducing agent is added dropwise at a constant temperature until the configured reducing agent is completely added to the reactor. The total amount of reducing agent added is 0.05 parts. The temperature of the reactor is gradually raised to 50°C, 60°C and 70°C for one hour each, and nitrogen filling is stopped. The emulsion that has reacted completely is poured into the distillation reactor, and the temperature is maintained at 70°C-80°C and distilled under reduced pressure to a concentration of 68.5%. 1.4% of a phase inversion agent is added to the distillation reaction to invert the phase, and a super-high concentration cationic emulsion polymer product with a molecular weight of 11.65 million, a bulk viscosity of 1783cp and a concentration of 67.5% is obtained.
[0066] Example 4
[0067] 280 parts of organic solvent, 3 parts of composite surfactant, 1.5 parts of self-made amphiphilic polymer stabilizer and 0.08 parts of oil-soluble initiator are added to the oil phase batching tank and stirred to dissolve; 220 parts of acrylamide monomer, 150 parts of cationic monomer, 0.06 parts of complexing agent, 0.07 parts of composite water-soluble initiator system and deionized water are added to the water phase tank and stirred to dissolve; the materials in the water phase tank are slowly pumped into the oil phase tank while stirring, and emulsified for 15 minutes with an emulsifier. After the particle size is tested to be qualified, the emulsified emulsion is pumped into the reactor, stirred and filled with nitrogen for more than 1 hour; the temperature of the reactor is reduced to 15°C with cooling brine, and nitrogen is continued to be filled; a solution with a reducing agent concentration of 1.8% is prepared, and oil and emulsifier are added for emulsification for standby use, the reducing agent is slowly added dropwise to the reactor with a metering pump, and the reducing agent dropping speed is adjusted according to the temperature rise. When the temperature of the reactor reaches 40°C, the reducing agent is added dropwise at a constant temperature until the configured reducing agent is completely added to the reactor. The total amount of reducing agent added is 0.06 parts. The temperature of the reactor is gradually raised to 50°C, 60°C and 70°C for one hour each, and nitrogen filling is stopped. The emulsion that has reacted completely is poured into the distillation reactor, and the temperature is maintained at 70°C-80°C and distilled under reduced pressure to a concentration of 67.2%. 1.2% of the phase inversion agent is added to the distillation reaction to invert the phase, and a super-high concentration cationic emulsion polymer product with a molecular weight of 9.88 million, a bulk viscosity of 1768cp and a concentration of 66.4% is obtained.
[0068] Example 5
[0069] 290 parts of organic solvent, 2.5 parts of composite surfactant, 2 parts of self-made amphiphilic polymer stabilizer and 0.06 parts of oil-soluble initiator are added to the oil phase batching tank and stirred to dissolve; 240 parts of acrylamide monomer, 140 parts of cationic monomer, 0.06 parts of complexing agent, 0.08 parts of composite water-soluble initiator system and deionized water are added to the water phase tank and stirred to dissolve; the materials in the water phase tank are slowly pumped into the oil phase tank while stirring, and emulsified for 15 minutes with an emulsifier. After the particle size is tested to be qualified, the emulsified emulsion is pumped into the reactor, stirred and filled with nitrogen for more than 1 hour; the temperature of the reactor is reduced to 15°C with cooling brine, and nitrogen is continued to be filled; a solution with a reducing agent concentration of 2% is prepared, and oil and emulsifier are added for emulsification for standby use, the reducing agent is slowly added dropwise to the reactor with a metering pump, and the initiator dropping speed is adjusted according to the temperature rise. When the temperature of the reactor reaches 40°C, the reducing agent is added dropwise at a constant temperature until the configured reducing agent is completely added to the reactor. The total amount of reducing agent added is 0.06 parts. The temperature of the reactor is gradually raised to 50°C, 60°C and 70°C for one hour each, and nitrogen filling is stopped. The emulsion that has reacted completely is poured into the distillation reactor, and the temperature is maintained at 70°C-80°C and distilled under reduced pressure to a concentration of 68.3%. 1% of a phase inversion agent is added to the distillation reaction to invert the phase, and a super-high concentration cationic emulsion polymer product with a molecular weight of 9.56 million, a bulk viscosity of 1820cp and a concentration of 67.6% is obtained.
[0070] Example 6
[0071] 290 parts of organic solvent, 2 parts of composite surfactant, 1 part of self-made amphiphilic polymer stabilizer, 0.08 parts of oil-soluble initiator are added to the oil phase batching tank and stirred thoroughly to dissolve; 230 parts of acrylamide monomer, 150 parts of cationic monomer, 0.06 parts of complexing agent, 0.07 parts of composite water-soluble initiator system and deionized water are added to the water phase tank and stirred thoroughly to dissolve; the materials in the water phase tank are slowly pumped into the oil phase tank while stirring, and emulsified for 15 minutes with an emulsifier, and after the particle size is tested to be qualified, the emulsified emulsion is pumped into the reactor, stirring is started, and nitrogen is filled for more than 1 hour; the temperature of the reactor is reduced to 15°C with cooling brine, and nitrogen is continued to be filled; a solution with a reducing agent concentration of 1.7% is prepared, and oil and emulsifier are added for emulsification for standby use, the initiator is slowly added dropwise to the reactor with a metering pump, and the initiator dropping speed is adjusted according to the temperature rise. When the temperature of the reactor reaches 40°C, add the reducing agent at a constant temperature until the configured reducing agent is completely added to the reactor. The total amount of reducing agent added is 0.05 parts. The temperature of the reactor is gradually raised to 50°C, 60°C and 70°C for one hour each, and the nitrogen filling is stopped. The emulsion that has reacted completely is poured into the distillation reactor and maintained at 70°C-80°C for reduced pressure distillation to a concentration of 66.7%. 1% of the phase inversion agent is added to the distillation reaction to invert the phase, and an ultra-high concentration cationic emulsion polymer product with a molecular weight of 11.5 million, a bulk viscosity of 1585cp and a concentration of 65.4% is obtained.
[0072] Example 7
[0073] 280 parts of organic solvent, 3 parts of composite surfactant, 1 part of self-made amphiphilic polymer stabilizer, 0.09 parts of oil-soluble initiator are added to the oil phase batching tank and stirred to dissolve; 210 parts of acrylamide monomer, 160 parts of cationic monomer, 0.07 parts of complexing agent, 0.08 parts of composite water-soluble initiator system and deionized water are added to the water phase tank and stirred to dissolve; the materials in the water phase tank are slowly pumped into the oil phase tank while stirring, and emulsified for 15 minutes with an emulsifier, and after the particle size is tested to be qualified, the emulsified emulsion is pumped into the reactor, stirring is started, and nitrogen is filled for more than 1 hour; the temperature of the reactor is reduced to 15°C with cooling brine, and nitrogen is continued to be filled; a solution with a reducing agent concentration of 1.8% is prepared, and oil and emulsifier are added for emulsification for standby use, the initiator is slowly added dropwise to the reactor with a metering pump, and the initiator dropping speed is adjusted according to the temperature rise. When the temperature of the reactor reaches 40°C, the reducing agent is added dropwise at a constant temperature until the configured reducing agent is completely added to the reactor. The total amount of reducing agent added is 0.06 parts. The temperature of the reactor is gradually raised to 50°C, 60°C and 70°C for one hour each, and nitrogen filling is stopped. The emulsion that has reacted completely is poured into the distillation reactor, and the temperature is maintained at 70°C-80°C and distilled under reduced pressure to a concentration of 66.9%. 1.2% of a phase inversion agent is added to the distillation reaction to invert the phase, and a super-high concentration cationic emulsion polymer product with a molecular weight of 9.07 million, a bulk viscosity of 1765cp and a concentration of 65.5% is obtained.
[0074] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0075] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing an ultra-high concentration cationic emulsion polymer flocculant, characterized in that: The steps include: Step 1, adding an organic solvent, a composite surfactant, a self-made polymer stabilizer and an oil-soluble initiator into an oil phase batching tank, stirring and dissolving them fully; Step 2, adding acrylamide monomer, cationic monomer, complexing agent, composite water-soluble initiator system and deionized water into a water phase tank and stirring to fully dissolve; Step 3, slowly pump the material in the water phase tank into the oil phase tank, stir the material in the oil phase tank during the pumping process, and then use an emulsifier to emulsify the material in the oil phase tank for 15 minutes. After the particle size is tested to be qualified, the emulsified emulsion is pumped into the reactor, stirring is started, and nitrogen is filled for more than 1 hour; Step 4: Use cooling brine to lower the temperature of the reactor to 15°C and continue to charge with nitrogen; Step 5: Prepare the reducing agent solution, add oil and emulsifier, and emulsify with an emulsifier for standby use; slowly drop the reducing agent solution into the reactor with a metering pump, and adjust the reducing agent dropping speed according to the temperature rise; Step 6, when the temperature of the reactor reaches 40°C, add the initiator dropwise at a constant temperature until the configured initiator is completely added to the reactor, raise the temperature of the reactor step by step to 50°C, 60°C and 70°C, react for one hour respectively, and then stop nitrogen filling; Step 7, the emulsion after the reaction is completed is poured into a distillation reactor, and the temperature is maintained at 70°C-80°C and the vacuum distillation is performed to an effective concentration of ≥66.5%; Step 8, adding 1%-1.5% of a phase inversion agent to the distillation reaction to invert the phase, to obtain an ultra-high concentration cationic emulsion polymer product with a concentration of ≥65%; The self-made polymer stabilizer is a copolymer of any two monomers of tetradecyl acrylate, hexadecyl acrylate, octadecyl acrylate and behenyl acrylate, the monomer compounding ratio is 1:1, and the viscosity of a 40% solution of the polymer stabilizer is required to be 300-800cp.
2. The method for preparing the ultra-high concentration cationic emulsion polymer flocculant according to claim 1, characterized in that: The organic solvent is white oil and D60 solvent oil in a ratio of 1:3; The composite surfactant is any two of span85, span80, and span60, with a weight ratio of 1:1, and after mixing, is compounded with any one of Tween80 and Tween81, with a compound weight ratio of 1:
1.
3. The method for preparing the ultra-high concentration cationic emulsion polymer flocculant according to claim 1, characterized in that: The oil-soluble initiator is a compound of azobisisobutyronitrile and azobisisovaleronitrile, and the weight ratio is 1:
2.
4. The method for preparing the ultra-high concentration cationic emulsion polymer flocculant according to claim 1, characterized in that: The cationic monomer is one or both of acryloyloxyethyl trimethyl ammonium chloride and methacrylamide ethyl trimethyl ammonium chloride; The complexing agent is one or more of sodium ethylenediaminetetraacetate, sodium ethylenediaminetetrapropionate, and sodium diethylenetriaminepentaacetate.
5. The method for preparing the ultra-high concentration cationic emulsion polymer flocculant according to claim 1, characterized in that: The composite water-soluble initiator system comprises ammonium persulfate, azobisisobutylimidazoline hydrochloride and azobisisobutylamidine hydrochloride, and the ratio of the three initiators is 3:1:
1.
6. The method for preparing the ultra-high concentration cationic emulsion polymer flocculant according to claim 1, characterized in that: The reducing agent concentration is 1.5%-2%; the reducing agent is one or more of sodium bisulfite, sodium sulfite and sodium pyrosulfite.
7. The method for preparing the ultra-high concentration cationic emulsion polymer flocculant according to claim 1, characterized in that: The phase transfer agent is any two of nonylphenol polyoxyethylene ether, octylphenol polyoxyethylene ether and polyoxyethylene ether natural fatty alcohol, and the ratio is 1:
1.
8. The method for preparing the ultra-high concentration cationic emulsion polymer flocculant according to claim 1, characterized in that: The polymer raw material, calculated by weight, includes the following components: 280-290 parts of organic solvent, 2-3 parts of composite surfactant, 1-2 parts of homemade polymer stabilizer, 0.05-0.1 parts of oil-soluble initiator, 210-240 parts of acrylamide monomer, 140-160 parts of cationic monomer, 0.05-0.08 parts of complexing agent, 0.07-0.08 parts of composite water-soluble initiator system and 0.05-0.06 parts of reducing agent.
9. An ultra-high concentration cationic emulsion polymer flocculant, characterized in that: The ultra-high concentration cationic emulsion polymer flocculant prepared by the method for preparing an ultra-high concentration cationic emulsion polymer flocculant according to any one of claims 1 to 8 has a concentration of ≥65%.
10. The ultra-high concentration cationic emulsion polymer flocculant according to claim 9, characterized in that: The molecular weight of the emulsion polymer flocculant is higher than 8 million.