A high-performance environmentally friendly microemulsion cutting fluid

By using specific proportions of ingredients and preparation processes in microemulsion cutting fluids, rust prevention, lubrication and stability are improved, solving the problems of insufficient performance and non-environmental protection of microemulsion cutting fluids in the existing technology, and achieving high performance and environmental protection. Development of micro-emulsion cutting fluid.

CN116751623BActive Publication Date: 2024-10-11INTELLIGENT MFG INST OF HFUT
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310789083.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-30
Publication Date
2024-10-11
Estimated Expiration
2043-06-30

AI Technical Summary

Technical Problem

Existing microemulsion cutting fluids have deficiencies in anti-rust performance, lubrication performance and stability, and their ingredients are not environmentally friendly, making it difficult to meet the high performance requirements of modern metal processing.

Method used

Using rapeseed oil, complex polybasic acid, alcohol amine additives, sorbitan monostearate, castor oil polyoxyethylene ether-12, tall oil fatty acid amide, complex ester lubricants, nano-black phosphorus additives and modified It is a high-performance and environmentally friendly microemulsion cutting fluid composed of silicone polyether defoamer and other materials. Through specific proportions and preparation processes, the synergistic effect of the components is achieved to improve rust prevention, lubrication and stability.

Benefits of technology

It significantly improves the anti-rust performance of ferrous metals and copper-based metals, reduces the friction coefficient, enhances the stability and extreme pressure performance of the cutting fluid, and the cutting fluid is biodegradable and meets the environmental protection requirements of modern industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004313111220000071
    Figure BDA0004313111220000071
  • Figure HDA0004313111230000011
    Figure HDA0004313111230000011
  • Figure HDA0004313111230000012
    Figure HDA0004313111230000012
Patent Text Reader

Abstract

The invention discloses a high-performance environmentally friendly microemulsion cutting fluid, which is composed of 14-20% rapeseed oil, 6-9% composite polyacid, 8-15% alcohol amine additives, 3-8% sorbitan monostearate, 6-11% castor oil polyoxyethylene ether-12, 1-2% tall oil fatty acid amide, 8-14% composite ester lubricant, 0.1-0.5% benzotriazole, 0.2-0.4% nano black phosphorus additive, 0.1-0.3% modified silicon polyether defoamer, and the rest is water. The present invention improves the dispersibility of additives, exerts a multi-component synergistic effect, realizes the synergistic enhancement of cutting fluid stability, lubricity, rust resistance and bactericidal performance, and the cutting fluid is easy to degrade and treat, meets the requirements of green processing, and has good application prospects in a variety of metal processing lubrication fields.
Need to check novelty before this filing date? Find Prior Art

Description

1. Technical Field

[0001] The invention relates to a lubricant for metal processing, in particular to an environmentally friendly microemulsion cutting fluid for metal processing. 2. Background Technology

[0002] Cutting fluid plays the role of lubrication, cooling, cleaning and rust prevention in the metal cutting process. It can effectively reduce the friction coefficient, improve the tool life and processing accuracy. At present, cutting fluids are mainly divided into water-based cutting fluids, oil-based cutting fluids and microemulsion cutting fluids. Among them, the anti-rust and lubrication properties of water-based cutting fluids are relatively weak, while the cooling and cleaning properties of oil-based cutting fluids need to be improved, so their application scope is subject to some restrictions. Relatively speaking, microemulsion cutting fluids have both the better cooling and cleaning properties of water-based cutting fluids and the better rust prevention and lubrication properties of oil-based cutting fluids, and have received widespread attention.

[0003] The commonly used microemulsion cutting fluids contain mineral oil, sodium nitrite, phenol, formaldehyde, heavy metals and other ingredients, which cannot meet the requirements for green processing, and the function of the microemulsion cutting fluid is achieved by various additives, but the dispersibility of the additives is not good, resulting in poor stability of the cutting fluid. An environmentally friendly microemulsion cutting fluid (CN115651744A) previously developed by the applicant is designed based on environmental protection issues and has achieved good results. However, with the improvement of metal processing requirements, higher requirements are put forward for the performance of the cutting fluid. In particular, since there are many additive components in the cutting fluid, the functions of the components should not only not affect each other, but also play a synergistic role. Therefore, it is necessary to develop a new high-performance environmentally friendly microemulsion cutting fluid product. III. Summary of the invention

[0004] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a high-performance environmentally friendly microemulsion cutting fluid to achieve the invention goals of improving rust resistance, reducing friction coefficient, enhancing stability and being more environmentally friendly.

[0005] The present invention is achieved through the following technical solutions:

[0006] A high-performance environmentally friendly microemulsion cutting fluid, which is composed by weight as follows: 14-20% rapeseed oil, 6-9% composite polyacid, 8-15% alcoholamine additives, 3-8% sorbitan monostearate, 6-11% castor oil polyoxyethylene ether-12, 1-2% tall oil fatty acid amide, 8-14% composite ester lubricant, 0.1-0.5% benzotriazole, 0.2-0.4% nano black phosphorus additive, 0.1-0.3% modified silicon polyether defoamer, and the rest is water, totaling 100%; wherein the composite polyacid is a compound of a dibasic acid and a tribasic acid in a mass ratio of 1:2.1-2.6; the alcoholamine additive is a compound of monoethanolamine and triethanolamine in a mass ratio of 1:4; and the composite ester lubricant is a compound of an amino acid ester and a diethanolamine borate in a mass ratio of 1:1.8-2.3.

[0007] Furthermore, the tribasic acid is 2,4,6-tris(aminocaproyl)-1,3,5-triazine.

[0008] Furthermore, the dibasic acid is one of dodecanedioic acid, phthalic acid and eicosaldeoic acid.

[0009] Furthermore, the nano black phosphorus is a flake structure with an average flake diameter of 70-110 nm.

[0010] Furthermore, the cutting fluid is prepared by the following steps:

[0011] Step 1, add water to the reactor, stir at a speed of 200-300r / min, heat to 35-45°C, mix the dibasic acid and the tribasic acid and add them to the reactor after ball milling, stir for 5-10 minutes, then heat the solution to 60°C, slowly add triethanolamine to the reactor, drip it in 5-8 minutes, stir and react for 5-15 minutes, and obtain solution A;

[0012] Step 2, add rapeseed oil to another reaction kettle, heat to 50-65°C, stir at 250-400r / min, slowly add the composite ester lubricant prepared in step 1, stir for 10-15 minutes, slowly add solution A prepared in step 1, stir for 5-10 minutes, add tall oil fatty acid amide, monoethanolamine, castor oil polyoxyethylene ether-12, and sorbitan monostearate in sequence, stir for 10-25 minutes, and obtain microemulsified solution B;

[0013] Step 3: Heat the solution B in step 2 to 65-75°C, stir at 200-300r / min, add the nano black phosphorus additive, stir for 30-40 minutes, stop heating, continue stirring until the temperature drops to room temperature, add benzotriazole and modified silicone polyether defoamer in sequence, stir for 10-15 minutes, and obtain the cutting fluid.

[0014] Compared with the prior art, the present invention has the following beneficial effects:

[0015] 1. The present invention adopts polyacid triethanolamine ester, benzotriazole and amino acid ester and diethanolamine borate in a specific ratio generated by the reaction of polyacid and triethanolamine, which can play a good synergistic lubrication role and can achieve the anti-rust performance of ferrous metals and copper-based metals above Class B; through the synergistic effect between ester lubricants and polyacid triethanolamine esters, the lubrication and extreme pressure properties of the cutting fluid can be improved, wherein the friction coefficient can reach below 0.06, and the extreme pressure value can reach above 1500N.

[0016] 2. The present invention optimizes the components of the cutting fluid and adopts a unique preparation process to prepare the microemulsion cutting fluid, wherein monoethanolamine, triethanolamine and nano black phosphorus additives can synergistically improve the bactericidal performance of the cutting fluid, exerting a one-dose multi-effect effect, without the need to add additional bactericides, and can be processed and recycled for more than 2 months without deterioration or odor.

[0017] 3. The present invention effectively promotes the formation of solution A through mixed ball milling, and then synergistically promotes the formation of microemulsion with tall oil fatty acid amide and ester additives. The cutting fluid will not become turbid, stratified or precipitated after being left standing for more than 6 months, and has strong storage stability.

[0018] 4. The microemulsion cutting fluid components of the present invention are biodegradable, green and environmentally friendly, and meet the environmental protection requirements of modern machinery manufacturing, electronic and electrical industry, and aerospace industry for metal processing cutting fluids. IV. Description of the drawings

[0019] Figure 1 The figure is a comparison chart of the stability performance of Example 5 and Comparative Examples 1, 2, and 3.

[0020] Figure 2 It is a comparison chart of the antirust performance of Example 5 and Comparative Examples 1, 2, and 3.

[0021] Figure 3 The figure is a comparison chart of the bactericidal performance of Example 5 and Comparative Examples 1, 2, and 3. V. Specific implementation methods

[0022] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] The composite polyacid used in Examples 1-5 is a composite of dodecanedioic acid and 2,4,6-tris(aminocaproic acid)-1,3,5-triazine in a mass ratio of 1:2.3; the composite ester lubricant is a composite of amino acid ester and diethanolamine borate in a mass ratio of 1:1.95; the nano additive is nano black phosphorus, which has a flaky structure and an average flake diameter of 70-110 nm.

[0024] Embodiment 1:

[0025] The mass percentages of the high performance and environmentally friendly microemulsion cutting fluid of this embodiment are as follows:

[0026] Rapeseed oil 16%; complex polyacid 7%; alcoholamine additives 11%; dehydrated sorbitan monostearate 3%; castor oil polyoxyethylene ether-126.5%; tall oil fatty acid amide 1%; complex ester lubricant 10%; benzotriazole 0.1%; modified silicone polyether defoamer 0.1%; water balance.

[0027] The cutting fluid is prepared by the following preparation method:

[0028] (1) Add water to a reactor, stir at a speed of 300 r / min, heat to 45°C, mix and ball-mill the dibasic acid and the tribasic acid, add them to the reactor, stir for 10 minutes, then heat the solution to 60°C, slowly add triethanolamine to the reactor, drip it in 6 minutes, stir and react for 15 minutes, and obtain solution A;

[0029] (2) Add rapeseed oil to another reaction kettle, heat to 60° C., stir at 400 r / min, slowly add complex ester lubricant, stir for 15 minutes, slowly add solution A prepared in (1), stir for 5 minutes, add tall oil fatty acid amide, monoethanolamine, castor oil polyoxyethylene ether-12, and sorbitan monostearate in sequence, stir for 20 minutes, and obtain microemulsified solution B;

[0030] (3) Solution B in (2) was heated to 70° C., stirred at 300 r / min, and benzotriazole and modified silicone polyether defoamer were added in sequence, and stirred for 10 minutes to obtain the cutting fluid.

[0031] Embodiment 2:

[0032] The mass percentages of the high performance and environmentally friendly microemulsion cutting fluid of this embodiment are as follows:

[0033] Rapeseed oil 16%; complex polyacid 7%; alcoholamine additives 11%; dehydrated sorbitan monostearate 3%; castor oil polyoxyethylene ether-126.5%; tall oil fatty acid amide 1%; amino acid ester 3%; diethanolamine borate 7%; benzotriazole 0.1%; nano black phosphorus additive 0.2%; modified silicon polyether defoamer 0.1%; water balance.

[0034] The cutting fluid is prepared by the following preparation method:

[0035] (1) Add water to a reactor, stir at a speed of 300 r / min, heat to 45°C, mix and ball-mill the dibasic acid and the tribasic acid, add them to the reactor, stir for 10 minutes, then heat the solution to 60°C, slowly add triethanolamine to the reactor, drip it in 6 minutes, stir and react for 15 minutes, and obtain solution A;

[0036] (2) Add rapeseed oil to another reaction kettle, heat to 60° C., stir at 400 r / min, slowly add diethanolamine borate and amino acid ester, stir for 15 minutes, slowly add solution A prepared in (1), stir for 5 minutes, add tall oil fatty acid amide, monoethanolamine, castor oil polyoxyethylene ether-12, and sorbitan monostearate in sequence, stir for 20 minutes, and obtain microemulsified solution B;

[0037] (3) Solution B in (2) was heated to 70° C., stirred at 300 r / min, and nano black phosphorus was added. The mixture was stirred for 40 minutes. The heating was stopped, and the mixture was cooled to room temperature with continuous stirring. Benzotriazole and modified silicone polyether defoamer were added in sequence, and the mixture was stirred for 10 minutes to obtain the cutting fluid.

[0038] Embodiment 3:

[0039] The mass percentages of the high performance and environmentally friendly microemulsion cutting fluid of this embodiment are as follows:

[0040] Rapeseed oil 16%; complex polyacid 7%; alcoholamine additives 11%; dehydrated sorbitan monostearate 3%; castor oil polyoxyethylene ether-126.5%; tall oil fatty acid amide 1%; complex ester lubricant 10%; benzotriazole 0.1%; modified silicon polyether defoamer 0.1%; nano black phosphorus additive 0.2%; water balance.

[0041] The cutting fluid is prepared by the following preparation method:

[0042] (1) adding water to a reaction kettle, stirring at a speed of 300 r / min, heating to 45° C., adding a dibasic acid and a tribasic acid to the reaction kettle, stirring for 10 minutes, and then slowly adding triethanolamine to the reaction kettle, stirring and reacting for 15 minutes to obtain a solution A;

[0043] (2) adding rapeseed oil to another reaction kettle, heating to 60° C., stirring at 400 r / min, slowly adding complex ester lubricant, tall oil fatty acid amide, and monoethanolamine in sequence, stirring for 15 minutes, and obtaining solution B;

[0044] (3) Heat solution B in (2) to 65° C., stir at a speed of 300 r / min, add solution A, castor oil polyoxyethylene ether-12, and sorbitan monostearate, stir for 20 minutes, add nano black phosphorus, benzotriazole, and modified silicone polyether defoamer in sequence, and stir for 10 minutes to obtain the cutting fluid.

[0045] Embodiment 4:

[0046] The mass percentages of the high performance and environmentally friendly microemulsion cutting fluid of this embodiment are as follows:

[0047] Rapeseed oil 18%; complex polyacid 8%; alcoholamine additives 10%; dehydrated sorbitan monostearate 3.5%; castor oil polyoxyethylene ether-127.5%; tall oil fatty acid amide 1%; complex ester lubricant 8%; benzotriazole 0.1%; defoamer 0.2%; modified silicone polyether defoamer 0.3%; water balance

[0048] The cutting fluid is prepared by the following preparation method:

[0049] (1) Add water to a reactor, stir at a speed of 300 r / min, heat to 45°C, mix and ball-mill the dibasic acid and the tribasic acid, add them to the reactor, stir for 10 minutes, then heat the solution to 60°C, slowly add triethanolamine to the reactor, drip it in 6 minutes, stir and react for 15 minutes, and obtain solution A;

[0050] (2) Add rapeseed oil to another reaction kettle, heat to 60° C., stir at 400 r / min, slowly add the complex ester lubricant, stir for 15 minutes, slowly add the solution A prepared in (1), add tall oil fatty acid amide, monoethanolamine, castor oil polyoxyethylene ether-12, and sorbitan monostearate in sequence, stir for 20 minutes, and obtain a microemulsified solution B;

[0051] (3) Solution B in (2) was heated to 70° C., stirred at 300 r / min, and nano black phosphorus was added. The mixture was stirred for 40 minutes. The heating was stopped, and the mixture was cooled to room temperature with continuous stirring. Benzotriazole and modified silicone polyether defoamer were added in sequence, and the mixture was stirred for 10 minutes to obtain the cutting fluid.

[0052] Embodiment 5:

[0053] The mass percentages of the high performance and environmentally friendly microemulsion cutting fluid of this embodiment are as follows:

[0054] Rapeseed oil 16%; complex polyacid 7%; alcoholamine additives 11%; dehydrated sorbitan monostearate 3%; castor oil polyoxyethylene ether-126.5%; tall oil fatty acid amide 1%; complex ester lubricant 10%; benzotriazole 0.1%; modified silicon polyether defoamer 0.1%; nano black phosphorus additive 0.2%; water balance.

[0055] The cutting fluid is prepared by the following preparation method:

[0056] (1) Add water to a reactor, stir at a speed of 300 r / min, heat to 45°C, mix and ball-mill the dibasic acid and the tribasic acid, add them to the reactor, stir for 10 minutes, then heat the solution to 60°C, slowly add triethanolamine to the reactor, drip it in 6 minutes, stir and react for 15 minutes, and obtain solution A;

[0057] (2) Add rapeseed oil to another reaction kettle, heat to 60° C., stir at 400 r / min, slowly add the complex ester lubricant, stir for 15 minutes, slowly add the solution A prepared in (1), stir for 5 minutes, add tall oil fatty acid amide, monoethanolamine, castor oil polyoxyethylene ether-12, and sorbitan monostearate in sequence, stir for 20 minutes, and obtain microemulsion solution B;

[0058] (3) Solution B in (2) was heated to 70° C., stirred at 300 r / min, and nano black phosphorus was added. The mixture was stirred for 40 minutes. The heating was stopped, and the mixture was cooled to room temperature with continuous stirring. Benzotriazole and modified silicone polyether defoamer were added in sequence, and the mixture was stirred for 10 minutes to obtain the cutting fluid.

[0059] Comparative Example 1:

[0060] The mass percentages of the microemulsion cutting fluid in this comparative example are:

[0061] White oil 16%; tribasic acid 7%; triethanolamine 11%; white oil emulsifier 3.5%; tall oil 7%; borate rust inhibitor 12%; silicone defoamer 0.1%; BK fungicide 3%; water balance.

[0062] The cutting fluid is prepared by the following preparation method:

[0063] (1) Add water to a reaction kettle, stir at a speed of 300 r / min, heat to 50°C, add tribasic acid to water and stir until completely dissolved, slowly add triethanolamine to the reaction kettle, stir for 10 minutes after complete addition, and obtain solution A;

[0064] (2) Add white oil to solution A, heat to 60°C, stir at 300 r / min, add tall oil, borate rust inhibitor, white oil emulsifier, silicone defoamer, and BK bactericide in sequence, and continue stirring for 10 minutes to obtain a microemulsion cutting fluid.

[0065] Comparative Example 2:

[0066] The mass percentages of the microemulsion cutting fluid in this comparative example are:

[0067] White oil 12%; tribasic acid 5%; triethanolamine 14%; white oil emulsifier 3.5%; tall oil fatty acid amide 1%; ricinoleic acid polyester lubricant 6%; CP-50 rust inhibitor 12%; modified silicone polyether defoamer 0.1%; MBM fungicide 2%; water balance.

[0068] The cutting fluid is prepared by the following preparation method:

[0069] (1) Add water to a reactor, stir at 350 r / min, heat to 55°C, add tribasic acid to water and stir until completely dissolved, slowly add CP-50 rust inhibitor and triethanolamine to the reactor, stir for 15 minutes after complete addition, and obtain solution A;

[0070] (2) In another reaction kettle, heat to 60° C., stir at 300 r / min, add white oil, tall oil fatty acid amide, white oil emulsifier, and ricinoleic acid polyester lubricant in sequence, and continue stirring for 10 minutes to obtain solution B;

[0071] (3) Solution A in (1) was slowly added to solution B, heated to 60°C, stirred at 300 r / min for 15 minutes, and modified silicone polyether defoamer and MBM bactericide were added in sequence to obtain a microemulsion cutting fluid.

[0072] Comparative Example 3:

[0073] The mass percentages of the microemulsion cutting fluid in this comparative example are:

[0074] Castor oil 12%; fatty alcohol polyoxyethylene ether-306%; anionic surfactant 3.5%; composite organic rust inhibitor 25%; sodium tripolyphosphate 4%; polyether ester defoamer 0.02%; BK fungicide 3%; water balance.

[0075] The cutting fluid is prepared by the following preparation method:

[0076] (1) Castor oil and anionic surfactant were added into a reaction kettle respectively, stirred at a speed of 200 r / min, heated to 48° C., stirred for 5 minutes, and then allowed to stand and return to room temperature;

[0077] (2) Add 46% water to another reaction kettle and heat to 60° C., stir at 300 r / min, and slowly add fatty alcohol polyoxyethylene ether-30, sodium tripolyphosphate, composite organic rust inhibitor, polyether ester defoamer, and BK fungicide while stirring for 10 minutes;

[0078] (3) Using a long-necked funnel, slowly drip the solution obtained in step (1) into the reaction kettle in step (2), and stir at 60° C. and 200 r / min for 10 minutes, and let it stand to prepare a microemulsion cutting fluid.

[0079] The performance parameters of microemulsion cutting fluid are shown in Table 1.

[0080] Table 1 Microemulsion performance parameters

[0081]

[0082] Note: The actual measured conditions in the table are that carbide tools are used to process the surface of 45 steel shaft parts, the machine speed n = 1400r / min, the feed speed V f =1.87mm / s, feed rate f=0.08mm / r.

[0083] From the comparison of experimental data in Table 1, it can be seen that the present invention solves the current microemulsion cutting fluid comprehensive performance deficiency and environmental protection problems through the design of ingredients, new nano additives, the use of specific proportions of different ingredients and special processing technology. From Table 1, Examples 1-5 can meet the standard requirements in appearance, defoaming and storage stability. It can be seen that under the synergistic effect of polyacid triethanolamine ester, benzotriazole and amino acid ester and diethanolamine borate ester of specific proportion, Examples 1-5 can reach B grade or above in iron-based metal and copper-based metal corrosion experiments, compared with only D grade standard for copper-based alloy corrosion experiments in reference examples 1-3, and have obvious performance improvement. Under the synergistic effect of nano black phosphorus additives and different ester additives, Examples 1-5 can reach 1294N, 42Kg or more in extreme pressure and maximum no-calorie load, and the friction coefficient can reach 0.071 or less, compared with the friction coefficient of 510N, 36Kg and the lowest 0.081 in reference examples 1-3, and have more excellent tribological properties. It can better improve the processing quality and extend the service life of the tool, so that the tool replacement cycle is increased from the highest of 52 days in the control example to the lowest of 61 days in the embodiment. The combination of nano additives and alcohol amine additives effectively improves the bactericidal property of the cutting fluid, so that the continuous service life of the cutting fluid can reach more than 55 days.

Claims

1. A high-performance environmentally friendly microemulsion cutting fluid, characterized in that: The composition by mass percentage is as follows: 14-20% rapeseed oil, 6-9% composite polyacid, 8-15% alcoholamine additive, 3-8% sorbitan monostearate, 6-11% castor oil polyoxyethylene ether-12, 1-2% tall oil fatty acid amide, 8-14% composite ester lubricant, 0.1-0.5% benzotriazole, 0.2-0.4% nano black phosphorus additive, 0.1-0.3% modified silicon polyether defoamer, and the rest is water, totaling 100%; wherein the composite polyacid is a compound of dibasic acid and tribasic acid in a mass ratio of 1:2.1-2.6; the alcoholamine additive is a compound of monoethanolamine and triethanolamine in a mass ratio of 1:4; the composite ester lubricant is a compound of amino acid ester and diethanolamine borate in a mass ratio of 1:1.8-2.

3.

2. A high-performance environmentally friendly microemulsion cutting fluid according to claim 1, characterized in that: The tribasic acid is 2,4,6-tris(aminocaproyl)-1,3,5-triazine.

3. A high-performance environmentally friendly microemulsion cutting fluid according to claim 1, characterized in that: The dibasic acid is one of dodecanedioic acid, phthalic acid and eicosaldeoic acid.

4. A high-performance environmentally friendly microemulsion cutting fluid according to claim 1, characterized in that: The nano black phosphorus is a flake structure with an average flake diameter of 70-110 nm.

5. A high-performance environmentally friendly microemulsion cutting fluid according to claim 1, characterized in that: Prepared as follows: Step 1, add a given amount of water into a reactor, stir at a speed of 200-300 r / min, heat to 35-45°C, mix and ball-mill the dibasic acid and the tribasic acid, add them into the reactor, stir for 5-10 minutes, then heat the solution to 60°C, slowly add triethanolamine into the reactor, drip it in 5-8 minutes, stir and react for 5-15 minutes, and obtain solution A; Step 2, add rapeseed oil to another reaction kettle, heat to 50-65°C, stir at 250-400r / min, slowly add complex ester lubricant, stir for 10-15 minutes, slowly add solution A prepared in step 1, stir for 5-10 minutes, add tall oil fatty acid amide, monoethanolamine, castor oil polyoxyethylene ether-12, sorbitan monostearate in sequence, maintain 50-65°C, stir for 10-25 minutes, and obtain microemulsified solution B; Step 3: Heat the solution B in step 2 to 65-75°C, stir at 200-300r / min, add the nano black phosphorus additive, stir for 30-40 minutes, stop heating, continue stirring until the temperature drops to room temperature, add benzotriazole and modified silicone polyether defoamer in sequence, stir for 10-15 minutes, and obtain the cutting fluid.