An epitaxial method for reducing the surface roughness of silicon carbide homogeneous epitaxial wafer
By performing multi-step etching and buffer layer growth on the silicon carbide substrate, combining flow and pressure control, the problem of excessive surface roughness of the silicon carbide epitaxial sheet is solved, and lower surface roughness and higher devices are achieved Performance, suitable for the manufacturing of multi-layer small-size devices.
Patent Information
- Application Number
- CN202310556116.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-17
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-05-17
AI Technical Summary
In the prior art, the surface roughness of the silicon carbide homoepitaxial sheet is too large, resulting in subsequent device performance degradation, prolonged processing time and increased leakage current.
By placing a silicon carbide substrate on a graphite tray, the temperature and hydrogen flow in the reaction chamber are controlled, and the multi-step etching and buffer layer growth are performed, combined with flow and pressure control, the carbon-silicon ratio is gradually reduced to optimize the growth of the epitaxial layer. In-situ annealing and doping techniques are used to control surface roughness.
It effectively reduces the surface roughness of the silicon carbide homoepitaxial sheet, reduces warpage and subsequent CMP processing time, improves the flatness and production efficiency of the device, and is suitable for the manufacturing of multi-layer small-size devices.
Smart Images

Figure CN116770430B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an epitaxial method for reducing the surface roughness of a silicon carbide homogeneous epitaxial wafer, and belongs to the technical field of semiconductors. Background Art
[0002] In recent years, as an outstanding representative of wide bandgap semiconductor materials, silicon carbide has excellent properties such as wide bandgap width, high thermal conductivity, high breakdown electric field, high radiation resistance, and high electron saturation rate. High-frequency, high-voltage, and high-power devices based on silicon carbide materials are widely used in rail transportation, photovoltaics, industrial power supplies, etc. However, it is crucial to prepare high-quality epitaxial films that meet the performance requirements of devices. The surface roughness of epitaxial wafers is one of the key indicators that restrict the performance of subsequent devices. Excessive roughness will extend the processing time, increase the difficulty of device tape-out, and increase the leakage current of the device, which will eventually lead to performance degradation.
[0003] Based on the current prominent problem of excessive surface roughness of epitaxial wafers, the main reasons are analyzed as scratch damage on the substrate itself, abnormal obstruction of step flow growth due to falling objects, unstable growth process in the cavity environment, etc. Based on this situation, an epitaxial method to reduce the surface roughness of silicon carbide homogeneous epitaxial wafers is proposed. Summary of the invention
[0004] The object of the present invention is to provide an epitaxial method for reducing the surface roughness of a silicon carbide homogeneous epitaxial wafer, so as to solve the defect that the existing method makes the surface roughness of the epitaxial wafer too large.
[0005] An epitaxial method for reducing the surface roughness of a silicon carbide homogeneous epitaxial wafer, the method comprising:
[0006] S1: Place the silicon carbide substrate in the groove of the graphite tray, place the graphite tray on the graphite base of the reaction chamber, and close the hatch;
[0007] S2: Use inert gas to fill and pump the reaction chamber multiple times. After the evacuation is completed, set the main hydrogen volume to 10-40slm and the chamber pressure to 50mbar-100mbar;
[0008] S3: raising the temperature in the reaction chamber to a first preset temperature of 1450-1550° C., controlling the rotation of the tray to maintain 0.6-1.5 s / r, and annealing in the in-situ furnace for 5-10 min;
[0009] S4: Then continue to raise the temperature to the second preset temperature of 1550-1750° C., while increasing the hydrogen flow rate to 80-120 slm. When the second preset temperature is reached, the flow rate of carbon source / silicon source is coordinated to maintain the etching time for 5-30 min;
[0010] S5: After etching is completed, a carbon source and a silicon source are introduced to grow a buffer layer with a low C / Si ratio for 2-10 minutes using an epitaxial growth process;
[0011] S6: After the buffer layer is completed, a secondary etching is performed, and the etching time is maintained for 0-5 minutes; after the etching is completed, the appropriate C / Si ratio is maintained for 0-5 minutes, and then the amount of carbon source and silicon source is changed to turn to the growth of an epitaxial layer with a higher carbon-silicon ratio.
[0012] Furthermore, the main hydrogen volume is controlled by a flow controller MFC to control the hydrogen flow rate, thereby controlling the flow rate of the reaction chamber; the chamber pressure is achieved by controlling the opening angle of the butterfly valve.
[0013] Furthermore, in step S3, when the temperature is raised to a first preset temperature and is lower than the epitaxial temperature, in-situ etching is performed in the furnace for 5-10 minutes, wherein the first preset temperature is not lower than 1450°C.
[0014] Furthermore, in step S3, during the time from the first preset temperature of 1450°C to the second preset temperature of not less than 1550°C, the hydrogen flow rate is controlled by the mass flow meter MFC to increase to not less than 80slm. After reaching the second preset temperature, the etching rate is adjusted with the help of a carbon source of not more than 10sccm, so that the etching rate is not less than 0.02μm / min, and the etching time is maintained for 5-30min.
[0015] Furthermore, in the step S5, the growth process is used, and the overall epitaxy consists of a buffer layer and an epitaxial layer. After the etching is completed, the buffer layer growth is started, and the mass flow controller MFC is used to control the introduction of ethylene not higher than 50 sccm to control the carbon source introduction rate; at the same time, the temperature of the bubbler is set to 13-25°C and the pressure is 500mbar-800mbar. The mass flow controller MFC is used to control the carrier gas hydrogen to enter the bubbler to bring out the gaseous trichlorosilane, and then the flow pressure controller FPC is used to control the composition and flow rate of the trichlorosilane entering the reaction chamber to grow a buffer layer with a lower C / Si ratio not higher than 0.8, maintain a growth rate not higher than 0.15μm / min, and use N-type doping source nitrogen for doping to make its doping concentration 1-7E18cm-3 and the growth thickness 0.5-3.5μm.
[0016] Furthermore, in step S6, after the buffer layer is completed, the reaction source is changed from on to pre-on state, and a secondary etching is performed with an etching time of 0-5 minutes. After the etching is completed, the carbon-silicon ratio growth is continued for a maintenance time of 0-5 minutes. The carbon-silicon ratio is adjusted in a window between 0.8-1 to achieve a smooth transition from the buffer layer to the epitaxial layer.
[0017] Furthermore, the carbon-to-silicon ratio of the buffer layer can be adjusted within a window of 0.6-0.8.
[0018] Further, in the step S6, the epitaxial layer is grown, and the mass flow controller MFC is used to control the introduction of ethylene not higher than 200 sccm, thereby controlling the carbon source introduction rate; at the same time, the temperature of the bubbler is set to 13-25°C, and the pressure is 500mbar-800mbar, and the carrier gas hydrogen is controlled by the mass flow controller MFC to enter the bubbler to bring out the gaseous trichlorosilane, and then the flow pressure controller FPC is used to control the composition and flow rate of the trichlorosilane entering the reaction chamber, and an epitaxial layer with a high C / Si ratio of not less than 1 is grown, and a growth rate of not less than 0.25μm / μm is maintained, and N-type doping source nitrogen is used for doping to make its doping concentration 1-8E15cm -3 , the growth thickness is 10-60μm.
[0019] Furthermore, the hydrogen flow rate introduced into the bubbler is 30-150sccm, the pressure entering the cavity is 1500-2500mbar, and the trichlorosilane content actually introduced into the cavity is 30-150sccm; the ethylene content actually introduced into the cavity is 10-50sccm; the hydrogen flow rate introduced into the bubbler is 60-300sccm, the pressure entering the cavity is 1500-2500mbar, and the trichlorosilane content actually introduced into the cavity is 60-300sccm; the ethylene content actually introduced into the cavity is 40-200sccm.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] 1. The present invention can reduce the roughness of a single-point selected area within a range of 10×10μm to an extremely low level (Rq≤0.107nm), and the overall multi-point average can be reduced to below 0.2nm;
[0022] 2. The in-situ annealing of the present invention can also reduce the overall warping of the epitaxial wafer and reduce the CMP processing time after the epitaxial wafer without causing derivative problems, thus greatly benefiting the yield of multi-layer small-size devices;
[0023] 3. The effect of reducing roughness is more obvious as the thickness increases or the growth rate accelerates, which provides an effective method for reducing surface flatness during subsequent thick film epitaxy or rapid epitaxial growth. It also reduces the process development cycle and improves production efficiency without deteriorating parameters such as defects. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 A flow chart of the process steps of the method;
[0025] Figure 2 This method prepares a single-point surface atomic force map of an epitaxial wafer;
[0026] Figure 3 This method prepares multi-point surface atomic force images of epitaxial wafers. DETAILED DESCRIPTION
[0027] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further explained below in conjunction with specific implementation methods.
[0028] like Figure 1-Figure 3 As shown, an epitaxial method for reducing the surface roughness of a silicon carbide homogeneous epitaxial wafer is as follows:
[0029] S1: First, place the silicon carbide substrate in the groove of the graphite tray, then use the robot to slowly put it into the graphite base of the reaction chamber and close the door;
[0030] S2: Use inert gas to fill and pump the reaction chamber multiple times. After the evacuation is completed, set the main hydrogen volume to 10-40slm and the chamber pressure to 50mbar-100mbar;
[0031] S3: Then, the temperature in the reaction chamber is raised to a first preset temperature of 1450-1550° C., and the rotation of the tray is controlled to maintain 0.6-1.5 s / r, and the in-situ furnace annealing is performed for 5-10 min;
[0032] S4: Then continue to heat up to the second preset temperature of 1550-1750°C, while increasing the hydrogen flow rate to 80-120slm. When the second preset temperature is reached, a carbon source / silicon source with a very small flow rate is used to maintain the etching time for 5-30min;
[0033] S5: After etching is completed, a carbon source and a silicon source are immediately introduced to grow a buffer layer with a low C / Si ratio for 2-10 minutes using a standard epitaxial growth process;
[0034] S6: After the buffer layer is completed, a secondary etching is performed, and the etching time is maintained for 0-5 minutes; after the etching is completed, the appropriate C / Si ratio is maintained for 0-5 minutes;
[0035] S7: Then, changing the amount of the carbon source and the silicon source to grow an epitaxial layer with a higher carbon-silicon ratio;
[0036] S8: Finally, cool down to the temperature where the slices can be taken out and close the hydrogen valve.
[0037] Based on the current epitaxial scheme, in step S2, the main hydrogen volume 10-40slm is controlled by the flow controller MFC to control the hydrogen flow rate, thereby controlling the flow rate of the reaction chamber; the chamber pressure 50-100mbar is achieved by accurately controlling the opening angle of the butterfly valve;
[0038] To further describe step S3, the temperature is raised to a first preset temperature, which is lower than the actual epitaxial temperature, and annealed in situ in the furnace for 5-10 minutes, so that the internal stress of the substrate wafer is fully released, the substrate warping problem is alleviated, and a good foundation is provided for subsequent epitaxy. At the same time, the substrate wafer is also preliminarily etched on the surface to remove tiny dust particles on the surface to prevent two-dimensional nucleation and subsequent interference with step flow growth; wherein the first preset temperature is not lower than 1450°C.
[0039] Further, in step S4, during the time from the first preset temperature of 1450°C to the second preset temperature of not less than 1550°C, the hydrogen flow rate is controlled by the mass flow meter MFC to be increased to not less than 80slm. After reaching the second preset temperature, at the same time, a small flow carbon source (not higher than 10sccm) is used to slightly adjust the etching rate so that the etching rate is not less than 0.02μm / min, and the etching time is maintained for 5-30min, so as to avoid the negative impact caused by the large-scale regulation of hydrogen flow and temperature;
[0040] In further detail, step S5 uses a standard growth process. The overall epitaxy consists of a buffer layer and an epitaxial layer. After etching, the buffer layer is immediately grown. First, a mass flow controller MFC is used to control the introduction of a small flow rate of ethylene not exceeding 50 sccm, thereby controlling the carbon source introduction rate. At the same time, the temperature of the bubbler is set to 13-25°C and the pressure is 500mbar-800mbar. The mass flow controller MFC is used to control the carrier gas hydrogen to enter the bubbler to bring out gaseous trichlorosilane. Then, the flow pressure controller FPC is used to control the composition and flow rate of trichlorosilane entering the reaction chamber, and a low C / Si ratio of not more than 0.8 buffer layer growth is performed, and a growth rate of not more than 0.15μm / min is maintained. N-type doping source nitrogen is used for doping to achieve a doping concentration of 1-8E15cm -3 , the growth thickness is 10-60μm.
[0041] Further, in step S6, after the buffer layer is completed, the reaction source is changed from on to pre-on state, and other process conditions remain unchanged, and secondary etching is performed for 0-5 minutes. This step is mainly to remove particles on the surface of the buffer layer to make it smoother. In addition, after the etching is completed, the growth of the appropriate carbon-silicon ratio is continued for 0-5 minutes. The appropriate carbon-silicon ratio can be adjusted within the window of 0.8-1, and a smooth transition from the buffer layer to the epitaxial layer is achieved.
[0042] In step S7, the epitaxial layer is grown, and the mass flow controller MFC is used to control the introduction of ethylene at a rate not higher than 200 sccm, thereby controlling the carbon source introduction rate; at the same time, the temperature of the bubbler is set to 13-25°C, and the pressure is 500mbar-800mbar, and the carrier gas hydrogen is controlled by the mass flow controller MFC to enter the bubbler to bring out the gaseous trichlorosilane, and then the flow pressure controller FPC is used to control the composition and flow rate of the trichlorosilane entering the reaction chamber, and an epitaxial layer with a high C / Si ratio of not less than 1 is grown, and a growth rate of not less than 0.25μm / μm is maintained, and N-type doping source nitrogen is used for doping to make the doping concentration 1-8E15cm -3 , the growth thickness is 10-60μm;
[0043] To further describe step S5, with respect to the carbon-silicon ratio design of the buffer layer, the carbon-silicon ratio can be adjusted within a window of 0.6-0.8; the hydrogen flow rate introduced into the bubbler is 30-150sccm, the pressure entering the cavity is 1500-2500mbar, and the actual trichlorosilane content introduced into the cavity is 30-150sccm; the actual ethylene content introduced into the cavity is 10-50sccm; the hydrogen flow rate introduced into the bubbler is 60-300sccm, the pressure entering the cavity is 1500-2500mbar, and the actual trichlorosilane content introduced into the cavity is 60-300sccm; the actual ethylene content introduced into the cavity is 40-200sccm.
[0044] In step S6, a reaction source with a relatively large flow rate is introduced to grow an epitaxial layer with a relatively high carbon-silicon ratio: on the one hand, the ethylene flow rate is precisely controlled to be ≤200 sccm by a mass flow controller; on the other hand, the trichlorosilane gas is brought out of the bubbler by the carrier gas hydrogen, and the flow pressure controller is used to precisely control the trichlorosilane entering the cavity to be ≤300 sccm; N-type doping is performed, and the doping source is nitrogen, and the doping concentration is 1-8E15cm -3 , the growth thickness is 10-60μm.
[0045] In step S8, based on step S7, the growth reaction source valve is disconnected, the temperature is lowered to 600-800°C, the epitaxial wafer is taken out to the wafer transfer area by a robot, cooled to room temperature, and tested, inspected, cleaned, and packaged.
[0046] In the implementation steps, for step S5, the ethylene flow rate is 10-50 sccm; the trichlorosilane flow rate is 30-150 sccm;
[0047] In the implementation steps, for step S7, the ethylene flow rate is 40-200 sccm; the trichlorosilane flow rate is 60-300 sccm;
[0048] Combination Figure 2It can be seen that the single point surface roughness Rq value is 0.107nm. Figure 3 It can be seen that the average value of the multi-point surface roughness Rq is less than 0.2nm. For 60μm thick film epitaxy, this indicator is relatively excellent.
[0049] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. An epitaxial method for reducing the surface roughness of a silicon carbide homogeneous epitaxial wafer, It is characterized in that The method comprises: S1: Place the silicon carbide substrate in the groove of the graphite tray, place the graphite tray on the graphite base of the reaction chamber, and close the hatch; S2: Use inert gas to fill and pump the reaction chamber multiple times. After the evacuation is completed, set the main hydrogen volume to 10-40slm and the chamber pressure to 50mbar-100mbar; S3: raising the temperature in the reaction chamber to a first preset temperature of 1450-1550° C., controlling the rotation of the tray to maintain 0.6-1.5 s / r, and annealing in situ in the furnace for 5-10 min; S4: Then continue to raise the temperature to the second preset temperature of 1550-1750° C., while increasing the hydrogen flow rate to 80-120 slm. When the second preset temperature is reached, the flow rate of carbon source / silicon source is coordinated to maintain the etching time for 5-30 min; S5: After etching is completed, a carbon source and a silicon source are introduced to grow a buffer layer with a low C / Si ratio for 2-10 minutes using an epitaxial growth process; S6: After the buffer layer is completed, a secondary etching is performed, and the etching time is maintained for 0-5 minutes; after the etching is completed, the appropriate C / Si ratio is maintained for 0-5 minutes, and then the amount of carbon source and silicon source is changed to turn to the epitaxial layer growth with a higher carbon-silicon ratio; In step S3, when the temperature is raised to a first preset temperature and is lower than the epitaxial temperature, in-situ furnace etching is performed for 5-10 minutes; In the step S4, after reaching the second preset temperature, the etching rate is adjusted by adding a carbon source of no more than 10 sccm, so that the etching rate is no less than 0.02 μm / min; In the step S5, the overall epitaxy is composed of a buffer layer and an epitaxial layer by using a growth process, and the buffer layer is grown after etching is completed. The mass flow controller MFC is used to control the introduction of ethylene not higher than 50 sccm to control the carbon source introduction rate; at the same time, the temperature of the bubbler is set to 13-25°C and the pressure is 500mbar-800mbar. The mass flow controller MFC is used to control the carrier gas hydrogen to enter the bubbler to bring out gaseous trichlorosilane. Then, the flow pressure controller FPC is used to control the composition and flow rate of trichlorosilane entering the reaction chamber, and a low C / Si ratio of not higher than 0.8 buffer layer is grown, and a growth rate of not higher than 0.15μm / min is maintained. The N-type doping source nitrogen is used for doping to make the doping concentration 1-7E18cm -3 , the growth thickness is 0.5-3.5μm; In the step S6, the epitaxial layer is grown, and the mass flow controller MFC is used to control the introduction of ethylene not higher than 200 sccm, thereby controlling the carbon source introduction rate; at the same time, the temperature of the bubbler is set to 13-25°C, and the pressure is 500mbar-800mbar, and the carrier gas hydrogen is controlled by the mass flow controller MFC to enter the bubbler to bring out the gaseous trichlorosilane, and then the flow pressure controller FPC is used to control the composition and flow rate of the trichlorosilane entering the reaction chamber, and an epitaxial layer with a high C / Si ratio of not less than 1 is grown, and a growth rate of not less than 0.25μm / μm is maintained, and N-type doping source nitrogen is used for doping to make its doping concentration 1-8E15cm -3 , the growth thickness is 10-60μm; The hydrogen flow rate into the bubbler is 30-150 sccm, the pressure entering the cavity is 1500-2500 mbar, the actual trichlorosilane content entering the cavity is 30-150 sccm; the actual ethylene content entering the cavity is 10-50 sccm.
2. The epitaxial method for reducing the surface roughness of a silicon carbide homogeneous epitaxial wafer according to claim 1, It is characterized in that The main hydrogen volume is controlled by a flow controller MFC to control the hydrogen flow rate, thereby controlling the flow rate of the reaction chamber; the chamber pressure is achieved by controlling the opening angle of the butterfly valve.
3. The epitaxial method for reducing the surface roughness of a silicon carbide homogeneous epitaxial wafer according to claim 1, It is characterized in that In step S6, after the buffer layer is completed, the reaction source is changed from on to pre-on state, and secondary etching is performed with an etching time of 0-5 minutes. After the etching is completed, the carbon-silicon ratio growth is continued for a maintenance time of 0-5 minutes. The carbon-silicon ratio is adjusted within a window of 0.8-1 to achieve a smooth transition from the buffer layer to the epitaxial layer.
4. The epitaxial method for reducing the surface roughness of a silicon carbide homogeneous epitaxial wafer according to claim 3, It is characterized in that The carbon-to-silicon ratio of the buffer layer can be adjusted within a window of 0.6-0.8.