A universal ion membrane for flow batteries
By using tertiary aminated polyphenyls and halogenated alkanes with cross-linking active sites in their side chains to prepare anionic exchange resin membranes in flow batteries, the existing problems of complex separator design and strong specificity are solved, and a universal ion membrane is realized. The preparation improves the Coulombic efficiency and electrolyte stability of the battery, is suitable for a variety of flow batteries, and promotes the commercialization process of flow batteries.
Patent Information
- Application Number
- CN202310054445.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-03
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-02-03
AI Technical Summary
Existing flow battery separators are complex in design, high in cost and highly specialized, making it difficult to apply to different electrolyte systems, and especially have poor stability under acidic conditions, which limits the wide application of flow batteries.
The anionic exchange resin polymer is prepared by quaternization reaction of tertiary aminated polyphenylene containing cross-linking active sites in the side chain and halogenated alkanes, and is evenly coated on the PET base film to form a universal ionic membrane, which is suitable for Different types of flow batteries.
It breaks the traditional separator-specific design barriers, reduces manufacturing costs, improves the Coulombic efficiency of the battery and the stability of the electrolyte, extends the battery maintenance cycle, and significantly improves the vanadium blocking ability in the all-vanadium redox flow battery, and is suitable for organic , inorganic flow batteries to meet the needs of commercial applications.
Smart Images

Figure CN116779927B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of energy storage liquid flow batteries, and in particular relates to a universal ion membrane for liquid flow batteries. Background Art
[0002] With the continuous penetration of new energy sources such as wind and light, the global demand for large-scale energy storage is also growing, especially long-term energy storage. Among electrochemical energy storage technologies, flow batteries have the characteristics of high safety, long cycle life, deep discharge, and energy and power independence, and have broad application prospects in large-scale long-term energy storage.
[0003] The diaphragm is one of the key materials of liquid flow batteries. Its main function is to separate the electrolytes of the positive and negative electrodes and selectively pass conductive ions. Therefore, the research and development of the diaphragm often needs to be designed and optimized based on the electrolyte system. It is not only difficult to develop, has a long feedback cycle, but also has a high cost ratio. The current mainstream liquid flow battery system uses inorganic metal vanadium as the electrolyte and uses the Nafion membrane of DuPont in the United States. The membrane has high vanadium ion permeability and water mobility, and is expensive, becoming another factor restricting the further development of all-vanadium liquid flow batteries in addition to vanadium electrolytes. CN 102005554 provides a diaphragm for an all-vanadium liquid flow battery, wherein the diaphragm attaches a water-soluble metal salt to the pores of a porous composite membrane to reduce the permeability of vanadium ions and the water mobility. The preparation of the membrane requires multiple infiltration, exchange, and drying with the water-soluble metal salt, and the process is complicated and has not yet been commercialized. CN 103219533 A discloses a graphene composite ion exchange membrane for a liquid flow battery and a preparation method thereof. The sulfonated polymer is modified by introducing graphene and / or graphene derivatives. The two-dimensional sheet-structured graphene or graphene derivative can improve the stability of the composite ion exchange membrane through interaction with polymer molecules and can also act as an obstacle to the penetration of active substances in the composite ion exchange membrane. The single cell has a high conductivity at 60 mA / cm 2 Under these conditions, the coulombic efficiency reached 98.3% and the voltage efficiency was 86.7%, providing a new direction for the structure of ion exchange membranes. The above membranes are only applicable to all-vanadium liquid flow batteries and are not applicable to other batteries.
[0004] In recent years, organic liquid flow batteries have begun to develop because of their wide source of raw materials and high safety. CN114914508A discloses the use of a porous membrane in a neutral aqueous organic liquid flow battery. The membrane has high chemical stability and high ion selectivity in a neutral aqueous organic liquid flow battery, but the membrane cannot ensure structural integrity under acidic conditions and cannot be used in all-vanadium liquid flow batteries. Summary of the invention
[0005] In order to solve the above problems, the present invention discloses a universal ion membrane for a liquid flow battery. The preparation method of the universal ion membrane for a liquid flow battery comprises the following steps:
[0006] Step (1): a tertiary aminated polyphenyl having a cross-linking active site in the side chain is subjected to a quaternization reaction with a halogenated alkane, the solution after the reaction is precipitated in a precipitant at room temperature, and the precipitated material after washing with acetone is dried at 70° C. for 24 hours to obtain an anion exchange resin polymer;
[0007] Step (2): prepare a 20-26wt% dimethyl sulfoxide solution of an anion exchange resin polymer, stir and mix evenly and filter, and evenly coat the filtered resin solution on a PET base film through a coating device, and then dry it at 70°C-100°C through a drying system provided by the coating device, wherein the drying system uses electric heating, and the ion membrane after drying is rolled up to obtain a universal ion membrane for a liquid flow battery, wherein the cross-linking active site is a compound containing a carbon-carbon double bond; the halogenated hydrocarbon includes any one or more of methyl chloride, methyl bromide, and methyl iodide; and the molar ratio of the cross-linking active site to the halogenated hydrocarbon is 1:
[0008] 1~1:3, the quaternization reaction process needs to be stirred in the dark.
[0009] Furthermore, the compound containing a carbon-carbon double bond in step (1) is preferably styrene.
[0010] Furthermore, the halogenated hydrocarbon in step (1) is preferably methyl iodide.
[0011] Furthermore, in step (1), the molar ratio of the side chain containing cross-linking active sites to the halogenated hydrocarbon is preferably 1:1.5.
[0012] Furthermore, the quaternization reaction time in step (1) is 48 hours, and the reaction temperature is 20-35°C.
[0013] Furthermore, in step (1), the precipitant is acetone, and the solution after the reaction is precipitated in excess acetone.
[0014] Furthermore, in step (1), the volume ratio of the anion exchange resin polymer to the acetone is 1:10.
[0015] Furthermore, the universal ion membrane for liquid flow batteries can be used in any one or more of organic liquid flow batteries, organic-inorganic hybrid liquid flow batteries, and inorganic liquid flow batteries.
[0016] Furthermore, the conductive ions of the organic liquid flow battery include any one or more of chloride ions, carbonate ions, bicarbonate ions, phosphate ions, hydrogen phosphate ions, dihydrogen phosphate ions, nitrate ions, sulfate ions, and hydrogen sulfate ions.
[0017] Furthermore, the inorganic flow battery includes an all-vanadium flow battery, an all-iron flow battery, an iron /
[0018] Any one or more of chromium flow battery, zinc / bromine flow battery, zinc / iodine flow battery, zinc / nickel flow battery, zinc / air flow battery, zinc / iron flow battery, iron / vanadium flow battery.
[0019] The beneficial effects of the present invention are:
[0020] 1. The universal ion membrane for liquid flow batteries of the present invention breaks the design barrier of special membranes in traditional liquid flow batteries. At the same time, the manufacturing cost of the membrane is low and it is easy to mass produce, which will greatly promote the development of the liquid flow battery industry;
[0021] 2. The universal ion membrane for liquid flow batteries of the present invention improves the vanadium resistance in all-vanadium liquid flow batteries, and the battery coulomb efficiency reaches more than 99.5%. While reducing the battery self-discharge, it slows down the liquid surface migration of the positive and negative electrolytes, significantly reduces the battery capacity attenuation, and extends the battery maintenance cycle;
[0022] 3. The universal ion membrane for liquid flow batteries described in the present invention is used in the field of organic liquid flow batteries. It has high selectivity for conductive ions, low membrane resistance, high mechanical strength, good stability and low cost, meeting the needs of commercial applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 Schematic diagram of battery testing device for Examples 2 to 4 and Comparative Examples 1 to 4 of the present invention.
[0024] Figure 2 The self-discharge of the universal membrane for liquid flow battery described in the present invention in the application of all-vanadium liquid flow battery is compared with that when using a cation membrane. DETAILED DESCRIPTION
[0025] The present invention will be further explained below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the following specific embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention.
[0026] Example 1
[0027] This example is used to illustrate the preparation method of the universal membrane provided by the present invention.
[0028] 200g of polystyrene and 86g of iodomethane were subjected to quaternization reaction at a molar ratio of 1:1.5, and stirred at 20-30°C in the dark for 48h. After the reaction, the solution was added dropwise to a 10-fold volume of acetone solution and stirred for 24h, and the precipitate was collected at room temperature. The precipitate was washed with acetone and dried at 70°C for 24h to obtain an anion exchange resin polymer.
[0029] Dissolve the anion exchange resin polymer in 1400g of dimethyl sulfoxide solution, stir and mix evenly, and filter. The filtered resin liquid is evenly coated on the PET base film through a coating device, and then dried at 80°C by the coating device's own drying system. The drying system uses electric heating. The dried ion membrane is rolled up to obtain the finished product.
[0030] Example 2
[0031] This example is used to illustrate the application of the universal membrane in Example 1 in an organic liquid flow battery.
[0032] Reference Figure 1 As shown, Figure 1 The schematic diagram of the battery test device of Examples 2 to 4 and Comparative Examples 1 to 4 of the present invention; wherein the positive electrode electrolyte in the positive electrode storage tank is pumped into the positive electrode of the test cell by the positive electrode circulation pump, and the negative electrode electrolyte in the negative electrode storage tank is pumped into the negative electrode of the test cell by the negative electrode circulation pump, and the electrolyte is divided into positive and negative electrodes by the diaphragm in the cell to perform the corresponding battery charge and discharge reaction. The battery test is implemented using the Xinwei battery test system.
[0033] The steps of this example are as follows: a finished membrane (10 cm × 10 cm) of Example 1 is cut and placed in a 1 M NaCl aqueous solution for 24 hours, and then assembled on an active area of 50 cm 2 In the single cell, the thickness of the carbon felt is 4 mm, and the distance between the ion membrane and the bipolar plate is 3 mm. The positive electrode electrolyte is a 1.0 mol / L aqueous solution of 2,2,6,6-tetramethyl-4-(N,N,N-trimethylquaternary ammonium) piperidinyloxy free radical chloride, and the negative electrode electrolyte is a 1.0 mol / L aqueous solution of N,N'-dimethyl-4,4'-bipyridyl dichloride. 1 mol / L NaCl is added to the positive and negative electrodes as supporting electrolytes. The charge and discharge test was carried out according to the following procedure: constant current and constant voltage charge / constant current discharge, the current density is 100 mA cm -2 , the charging cut-off voltage is 1.5V and the discharging cut-off voltage is 0.9V.
[0034] Example 3
[0035] This example is used to illustrate the application of the universal membrane in Example 1 in an all-vanadium liquid flow battery.
[0036] The difference between this embodiment and embodiment 2 is that the positive and negative electrolytes are 1.6 mol / L V (IV) / V (III), and the supporting electrolyte is 3 mol / L sulfuric acid. The charge and discharge procedures are: constant current charge and discharge, the current density is 80 mA cm -2, the charging cut-off voltage is 1.55V, and the discharging cut-off voltage is 1V. After the charging and discharging are completed, the battery is fully charged and then set aside, and the voltage changes over time are recorded.
[0037] Example 4
[0038] Six finished membranes (10 cm × 10 cm) prepared in Example 1 were cut and placed in a 1 M NaCl aqueous solution for 24 hours, and then assembled on an active area of 50 × 6 cm 2 In the six-series battery stack, the thickness of the carbon felt is 4mm, and the distance between the ion membrane and the bipolar plate is 3mm. The positive electrode electrolyte is a 1.0mol / L aqueous solution of 2,2,6,6-tetramethyl-4-(N,N,N-trimethylquaternary ammonium) piperidinyloxy free radical chloride, and the negative electrode electrolyte is a 1.0mol / L aqueous solution of N,N'-dimethyl-4,4'-bipyridyl dichloride. 1mol / L NaCl is added to the positive and negative electrodes as supporting electrolytes. The charge and discharge test was carried out according to the following procedure: constant current and constant voltage charge / constant current discharge, the current density is 100mA·cm -2 , the charging cut-off voltage is 9V and the discharging cut-off voltage is 5.4V.
[0039] Comparative Example 1
[0040] The steps of this comparative example are as follows: a piece of commercial AMVN membrane (10 cm × 10 cm) produced by Asahi Glass Co., Ltd. of Japan was cut and placed in a 1M NaCl aqueous solution for 24 hours, and then assembled on an active area of 50 cm 2 In the single cell, the thickness of the carbon felt is 4 mm, and the distance between the ion membrane and the bipolar plate is 3 mm. The positive electrode electrolyte is a 1.0 mol / L aqueous solution of 2,2,6,6-tetramethyl-4-(N,N,N-trimethylquaternary ammonium) piperidinyloxy chloride, and the negative electrode electrolyte is a 1.0 mol / L aqueous solution of N,N'-dimethyl-4,4'-bipyridinium dichloride. 1 mol / L NaCl is added to the positive and negative electrodes as supporting electrolytes. The charge and discharge test was carried out according to the following procedure: constant current and constant voltage charge / constant current discharge, the current density is 50 mA cm -2 , the charging cut-off voltage is 1.5V and the discharging cut-off voltage is 0.9V.
[0041] Comparative Example 2
[0042] The steps of this comparative example are as follows: a commercial membrane FAA-3-PE-30 from Fumatech, Germany, was cut and placed in a 1M NaCl aqueous solution for 24 hours, and then assembled on an active area of 50 cm 2In the single cell, the thickness of the carbon felt is 4 mm, and the distance between the ion membrane and the bipolar plate is 3 mm. The positive electrode electrolyte is a 1.0 mol / L aqueous solution of 2,2,6,6-tetramethyl-4-(N,N,N-trimethylquaternary ammonium) piperidinyloxy free radical chloride, and the negative electrode electrolyte is a 1.0 mol / L aqueous solution of N,N'-dimethyl-4,4'-bipyridyl dichloride. 1 mol / L NaCl is added to the positive and negative electrodes as supporting electrolytes. The charge and discharge test was carried out according to the following procedure: constant current and constant voltage charge / constant current discharge, the current density is 100 mA cm -2 , the charging cut-off voltage is 1.5V and the discharging cut-off voltage is 0.9V.
[0043] Comparative Example 3
[0044] The steps of this comparative example are as follows: a piece of commercial membrane N212 (10 cm × 10 cm) from DuPont Company of the United States was cut and placed in a 1M NaCl aqueous solution for replacement for 24 hours, and then assembled on an active area of 50 cm 2 In the single cell, the thickness of the carbon felt is 4 mm, and the distance between the ion membrane and the bipolar plate is 3 mm. The positive and negative electrolytes are 1.6 mol / L V (IV) / V (III), and the supporting electrolyte is 3 mol / L sulfuric acid. The charge and discharge procedures are: constant current charge and discharge, and the current density is 80 mA cm -2 , the charging cut-off voltage is 1.55V, and the discharging cut-off voltage is 1V. After the charging and discharging are completed, the battery is fully charged and then set aside, and the voltage changes over time are recorded.
[0045] Comparative Example 4
[0046] Six pieces of commercial membrane AMVN (10 cm × 10 cm) from Asahi Glass Co., Ltd. were cut and placed in 1 M NaCl aqueous solution for 24 hours, and then assembled in an active area of 50 × 6 cm. 2 In the six-series battery stack, the thickness of the carbon felt is 4mm, and the distance between the ion membrane and the bipolar plate is 3mm. The positive electrode electrolyte is a 1.0mol / L aqueous solution of 2,2,6,6-tetramethyl-4-(N,N,N-trimethylquaternary ammonium) piperidinyloxy free radical chloride, and the negative electrode electrolyte is a 1.0mol / L aqueous solution of N,N'-dimethyl-4,4'-bipyridyl dichloride. 1mol / L NaCl is added to the positive and negative electrodes as supporting electrolytes. The charge and discharge test was carried out according to the following procedure: constant current and constant voltage charge / constant current discharge, the current density is 100mA·cm -2 , the charging cut-off voltage is 9V and the discharging cut-off voltage is 5.4V.
[0047] Table 1: Battery test results of Examples 2-4 and Comparative Examples 1-4.
[0048]
[0049] As can be seen from Table 1, the ion membrane prepared by the present invention has excellent performance in both organic liquid flow batteries and inorganic liquid flow batteries; compared with Example 1 and Example 2, Example 2 shows that the universal membrane of the present invention has higher energy efficiency, capacity utilization and capacity retention in organic systems; compared with Example 3, Example 3 shows that the coulombic efficiency, capacity utilization and capacity retention of the universal membrane of the present invention in all-vanadium liquid flow batteries are significantly improved compared with the use of cation membranes, which greatly improves the electrolyte life of all-vanadium liquid flow batteries and prolongs the maintenance cycle. In addition, referring to Figure 2 As shown, after the battery is charged, the self-discharge rate in the battery is extremely slow (250 hours) using the universal membrane of the present invention. Under the same conditions, the battery using the positive membrane has been fully discharged within 50 hours. Example 4 is a 6-string amplification of Example 2. Its coulombic efficiency, energy efficiency, capacity utilization rate and capacity retention rate are better than those of Comparative Example 4, indicating that the universal membrane of the present invention has the same excellent performance in the amplification experiment. The universal membrane of the present invention has broad application prospects and will accelerate the commercialization process in the field of flow batteries.
[0050] It should be noted that the above content only illustrates the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications all fall within the protection scope of the claims of the present invention.
Claims
1. A universal ion membrane for a flow battery, characterized in that: The preparation method of the universal ion membrane for liquid flow battery is as follows: Step (1): a tertiary aminated polyphenyl having a cross-linking active site in the side chain is subjected to a quaternization reaction with a halogenated alkane, the solution after the reaction is precipitated in a precipitant at room temperature, the precipitated material after washing with acetone is dried at 70° C. for 24 hours to obtain an anion exchange resin polymer; Step (2): prepare a 20-26wt% dimethyl sulfoxide solution of an anion exchange resin polymer, stir and mix evenly and filter, and evenly coat the filtered resin solution on a PET base film through a coating device, and then dry it at 70°C-100°C through a drying system provided by the coating device, wherein the drying system uses electric heating, and the ion membrane after drying is rolled up to obtain a universal ion membrane for a liquid flow battery; the cross-linking active site is a compound containing a carbon-carbon double bond, and the compound containing a carbon-carbon double bond is styrene; the halogenated alkane includes any one or more of methyl chloride, methyl bromide, and methyl iodide; the molar ratio of the tertiary aminated polyphenylene containing a cross-linking active site on the side chain to the halogenated alkane is 1:1-1:3; and the quaternization reaction process needs to be stirred in the dark; The universal ion membrane for liquid flow batteries is used in any one or more of organic liquid flow batteries, organic-inorganic hybrid liquid flow batteries, and inorganic liquid flow batteries.
2. A universal ion membrane for a liquid flow battery according to claim 1, characterized in that: The halogenated alkane in step (1) is methyl iodide.
3. A universal ion membrane for a liquid flow battery according to claim 1, characterized in that: In step (1), the molar ratio of the tertiary aminated polyphenyl having a cross-linking active site in the side chain to the halogenated alkane is 1:1.
5.
4. A universal ion membrane for a liquid flow battery according to claim 1, characterized in that: The quaternization reaction time in step (1) is 48 hours, and the reaction temperature is 20-35°C.
5. A universal ion membrane for a liquid flow battery according to claim 1, characterized in that: In step (1), the precipitant is acetone, and the solution after the reaction is precipitated in excess acetone.
6. A universal ion membrane for a liquid flow battery according to claim 1, characterized in that: In step (1), the volume ratio of the anion exchange resin polymer to the acetone is 1:
10.
7. A universal ion membrane for a liquid flow battery according to claim 1, characterized in that: The conductive ions of the organic liquid flow battery include any one or more of chloride ions, carbonate ions, bicarbonate ions, phosphate ions, hydrogen phosphate ions, dihydrogen phosphate ions, nitrate ions, sulfate ions, and hydrogen sulfate ions.
8. A universal ion membrane for a liquid flow battery according to claim 1, characterized in that: The inorganic redox flow battery comprises an all-vanadium redox flow battery.