A method for preparing metal powder coating
By adopting low-speed stirring and interlayer preheating and cooling technology in the production of metal powder coatings, the problem of darker metal color and difference in finished powder effect in the bonding method is solved, and more efficient metal powder coating preparation and spraying effects are achieved.
Patent Information
- Application Number
- CN202310734724.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-20
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-06-20
AI Technical Summary
In the existing metal powder coating production technology, the bonding method results in a darker metal color and poor flash effect. In addition, the effect of different batches of finished powders varies greatly, and the process is complicated. The spraying process can easily block the gun.
Use low-speed stirring method to preheat the inner wall of the bonding machine, combined with interlayer heat transfer and cooling media to achieve uniform heating and rapid cooling, reduce the stirring speed to avoid violent impact of powder, add alumina to prevent agglomeration, and optimize the pigment and base Powder particle size and component proportions.
It improves the bonding efficiency of metal powder coatings and the metallic color consistency of finished powders, simplifies the process, and ensures the effect consistency and spraying effect uniformity of different batches of finished powders.
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing metal powder coating, and belongs to the technical field of powder coating preparation. Background Art
[0002] Metal powder coating refers to various powder coatings containing metal pigments (such as copper and gold powder, silver and aluminum powder, etc.). The current production technologies of metal powder coating mainly include dry mixing, melt extrusion and heat bonding. The dry mixing method is simple to operate. It only requires mixing the base powder with the metal pigment and completing it through simple mechanical stirring. However, the method has problems such as uneven spraying effect and easy clogging of the gun during spraying construction. The melt extrusion method is consistent with the powder production process. The metal pigment is mixed with the powder base material, and then melt extruded by an extruder, crushed by tableting, and separated by grinding. Due to the shearing effect of the screw during the melt extrusion process, the two-dimensional plane of the metal pigment is twisted and broken, and the shiny surface is destroyed. At the same time, the high temperature and aerobic environment cause the metal pigment to oxidize, resulting in a dark metal color and failing to achieve the expected effect.
[0003] The thermal bonding method is to stir the base powder with the bonding machine stirring paddle to generate friction heat, and continue stirring until the temperature rises to the glass transition temperature (T g ) point, the auxiliary feeder adds metal pigment to bond the metal powder; the finished powder bonded by the method greatly improves the physical and chemical properties of the metal pigment and the base powder compared to the dry mixing method and the melt extrusion method, and avoids the disadvantage of inconsistent metal effects on the surface of the plate caused by factors such as voltage, gravity, and charge during the spraying process. However, the thermal bonding method in the prior art is mainly based on the high-speed stirring of the base powder by the propeller in the bonding kettle (the stirring speed is above 1000rpm), so that the base powder is heated by friction to reach the bonding temperature; at the same time, the high-speed stirring enables the powder to obtain higher kinetic energy, and when the temperature rises to T g When the powder is near the point, the powder itself will soften to a certain extent. Under the high-speed stirring of the stirring paddle, the high-temperature softened base powder violently hits the inner wall of the bonding machine, causing it to accumulate and harden around the bonding kettle wall, the upper cover, the exhaust port and the stirring paddle of the bonding machine; at this time, adding metallic pigments will inevitably make the metallic pigments adhere to the inner wall of the bonding kettle first, and the high-speed stirring process will undoubtedly cause the two-dimensional structure of the metallic pigments to be tortuous, which will make the metallic color of the bonded finished powder darker and the flash effect poor. In addition, the base powder softened by high-speed stirring and friction heating accumulates on the inner wall of the bonding kettle, which increases the actual content of the bonded metallic pigments, resulting in large differences in the effects of the finished powders between different bonding batches. Summary of the invention
[0004] In view of the defects existing in the prior art, one of the objects of the present invention is to provide a method for preparing metal powder coating, which solves the problems of dark metallic color of the bonded finished powder, poor flash effect, and large differences in the effects of the finished powder between different bonding batches. At the same time, the bonding efficiency of the metal powder coating is significantly improved and the bonding process is simplified.
[0005] The objectives of the present invention are achieved through the following technical solutions.
[0006] A method for preparing a metal powder coating, the method comprising the following steps:
[0007] (1) Add pigment and primer into the bonding machine;
[0008] The pigment is at least one of a metallic pigment and an imitation metallic pigment; the imitation metallic pigment is a pigment having a metallic luster;
[0009] The mass of the pigment is 3% to 8% of the mass of the base powder;
[0010] The base powder is a conventional base powder in the field of metal powder coatings;
[0011] (2) Introduce nitrogen protective gas into the bonding machine, set the low-speed stirring speed to 60 rpm to 600 rpm, and then evenly preheat the inner wall of the bonding kettle of the bonding machine. The preheating bonding temperature is (T g +10)℃~(T g +20)℃,T g is the glass transition temperature of the foundation powder;
[0012] (3) When the material temperature in the bonding machine reaches the preheating bonding temperature described in step (2), the bonding timing is started, and the bonding timing time is 180s to 600s;
[0013] (4) After the bonding process is completed, the material is discharged into a cooling kettle connected to the bonding kettle for rapid cooling to obtain metal bonding powder;
[0014] (5) Take out the metal bonding powder obtained in step (4), sieve it and add alumina to improve fluidization and prevent agglomeration; the mass of alumina added is 0.1% to 0.3% of the mass of the metal bonding powder to obtain a metal powder coating.
[0015] Preferably, the particle size of the metallic pigment or the imitation metallic pigment is 30 to 100 μm; the median particle size (D50) of the base material is 40 to 45 μm.
[0016] Preferably, in step (1), the metallic pigment is copper gold powder; the imitation metallic pigment is pearlescent pigment;
[0017] Taking the total mass of the base powder as 100%, the raw material components and their mass fractions are as follows: 70% polyester resin, 5% triglycidyl isocyanurate (TGIC), 1% leveling agent, 0.3% benzoin, and 23.7% pigments and fillers; the pigments and fillers are a mixture of barium sulfate, red iron oxide, phthalocyanine blue and titanium dioxide.
[0018] Preferably, an interlayer is provided between the inner wall and the outer wall of the bonding kettle of the bonding machine, and heat source water or heat source oil is introduced into the interlayer as a heat transfer medium to uniformly preheat the interlayer of the bonding machine, thereby heating the material in the bonding kettle.
[0019] Further preferably, in step (2), heat source water is introduced into the interlayer of the bonding kettle to uniformly preheat the interlayer of the bonding machine.
[0020] Further preferably, in step (4), the rapid cooling method is to set an interlayer on the outer wall of the cooling kettle, set a stirring device in the cooling kettle, and introduce cold source water or air flow into the interlayer as a cooling medium, so that the discharge of the bonding kettle (high temperature) is fully in contact with the outer wall of the cooling kettle (low temperature) under the action of stirring, thereby generating heat exchange and achieving rapid cooling.
[0021] Beneficial Effects
[0022] (1) The present invention provides a method for preparing metal powder coatings, wherein the method preheats the inner wall of a bonding kettle, thereby preheating the pigment and base powder in the bonding kettle, so that the base powder can reach the bonding temperature without being stirred at high speed by a propeller; the bonding time can be effectively shortened, and the rotation speed can be reduced, thereby overcoming the problem that the base powder softened at high temperature is violently impacted by high-speed stirring, and adhesion and accumulation and hardening occur around the cylinder wall, upper cover, exhaust port and stirring paddle of the bonding machine, thereby ensuring that the proportion of metal pigments in different bonding batches is consistent; at the same time, the method can effectively reduce the stirring speed, and the low-speed stirring method effectively avoids the destruction of the metal pigment morphology by the propeller, thereby improving the metallic color of the bonding finished powder and the consistency of the finished powder effects between different bonding batches, and effectively ensuring that the finished powder has good metallic pigment color.
[0023] (2) The present invention provides a method for preparing metal powder coatings, wherein an interlayer is provided between the inner wall and the outer wall of the bonding kettle of the bonding machine, and heat source water or heat source oil is introduced into the interlayer as a heat transfer medium to uniformly heat the material in the barrel of the bonding machine, thereby simplifying the operating procedures of the bonding process and making it convenient and quick.
[0024] (3) The present invention provides a method for preparing metal powder coatings, wherein an interlayer is arranged on the outer wall of a cooling kettle, a stirring device is arranged in the cooling kettle, and cold source water or air flow is introduced into the interlayer as a cooling medium. Under the action of stirring, the discharge of the bonding kettle (high temperature) is fully contacted with the outer wall of the cooling kettle (low temperature), heat exchange is generated, and rapid cooling is achieved, which is efficient and convenient.
[0025] (4) The present invention provides a method for preparing a metal powder coating, wherein the particle size of the pigment is preferably 30 to 100 μm; the median particle size (D50) of the base material is preferably 40 to 45 μm; the pigment of the particle size and the base material are more fully and evenly mixed when stirred at a low speed, the prepared metal powder coating has a stronger metallic feel, and the bonding effect between the pigment and the base powder is better. DETAILED DESCRIPTION
[0026] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention, wherein the methods are conventional methods unless otherwise specified, and the raw materials can be obtained from public commercial channels unless otherwise specified.
[0027] In the following embodiments:
[0028] The bonding machine is produced by Yantai Lingyu Powder Machinery Co., Ltd.
[0029] The polyester resin is P5021, Weihai Longcai New Materials Co., Ltd.
[0030] The leveling agent is WL588, Ningbo Weikai Chemical Co., Ltd.
[0031] The base powder is prepared by the following method:
[0032] (1) weighing the raw materials of each component of the base powder according to the mass percentage, and then adding them into a mixer for thorough stirring to obtain a uniformly mixed base powder raw material;
[0033] Taking the total mass of the base powder as 100%, the raw materials of each component and their mass fractions are as follows: 70% polyester resin, 5% triglycidyl isocyanurate (TGIC), 1% leveling agent, 0.3% benzoin, 23.7% pigment and filler, wherein the pigment and filler is a mixture of barium sulfate, red iron oxide, phthalocyanine blue and titanium dioxide;
[0034] (2) adding the base powder raw material into the extruder feeder, performing melt extrusion, tableting and crushing to obtain a tablet;
[0035] (3) The material pieces are further crushed, ground, and sieved to obtain a base powder product with a medium particle size (D50) of 40 to 45 μm. The glass transition temperature (T g ) is 57°C.
[0036] Example 1
[0037] A method for preparing a metal powder coating, the method comprising the following steps:
[0038] (1) Adding pigment and base powder into a bonding machine; the pigment is copper gold powder and pearlescent pigment, the particle size of the pigment is 30 to 100 μm, and the mass of the pigment is 3% of the mass of the base powder;
[0039] (2) nitrogen protective gas is introduced into the bonding machine, and the rotation speed of the low-speed stirring is set to 60 rpm; an interlayer is provided between the inner wall and the outer wall of the bonding kettle of the bonding machine, and heat source water is introduced into the interlayer as a heat transfer medium. The water temperature of the heat source water is maintained at 67-69° C., and the inner wall of the bonding kettle of the bonding machine is uniformly preheated, and the preheating bonding temperature is 67° C.;
[0040] (3) When the material temperature in the bonding machine reaches the preheating bonding temperature of 67° C. in step (2), the bonding timing is started, and the bonding timing time is 180 seconds;
[0041] (4) After the bonding process is completed, the material is discharged into a cooling kettle connected to the bonding kettle. The outer wall of the cooling kettle is provided with an interlayer, and a stirring device is provided in the cooling kettle. Cold source water is introduced into the interlayer as a cooling medium. Under the action of stirring, the material discharged from the bonding kettle is fully contacted with the outer wall of the cooling kettle to achieve rapid cooling and obtain metal bonding powder;
[0042] (5) Take out the metal bonding powder obtained in step (4), sieve it and add alumina to improve fluidization and prevent agglomeration; the mass of alumina added is 0.1% of the mass of the metal bonding powder to obtain a metal powder coating.
[0043] Example 2
[0044] A method for preparing a metal powder coating, the method comprising the following steps:
[0045] (1) Adding pigment and base powder into a bonding machine; the pigment is copper gold powder and pearlescent pigment, the particle size of the pigment is 30 to 100 μm, and the mass of the pigment is 6% of the mass of the base powder;
[0046] (2) nitrogen protective gas is introduced into the bonding machine, and the rotation speed of the low-speed stirring is set to 200 rpm; an interlayer is provided between the inner wall and the outer wall of the bonding kettle of the bonding machine, and heat source water is introduced into the interlayer as a heat transfer medium. The water temperature of the heat source water is maintained at 67-69° C., and the inner wall of the bonding kettle of the bonding machine is uniformly preheated, and the preheating bonding temperature is 67° C.;
[0047] (3) When the material temperature in the bonding machine reaches the preheating bonding temperature of 67° C. in step (2), the bonding timing is started, and the bonding timing time is 600 seconds;
[0048] (4) After the bonding process is completed, the material is discharged into a cooling kettle connected to the bonding kettle. The outer wall of the cooling kettle is provided with an interlayer, and a stirring device is provided in the cooling kettle. Air flow is introduced into the interlayer as a cooling medium. Under the action of stirring, the material discharged from the bonding kettle is fully contacted with the outer wall of the cooling kettle, so that rapid cooling is achieved to obtain metal bonding powder;
[0049] (5) Take out the metal bonding powder obtained in step (4), sieve it and add alumina to improve fluidization and prevent agglomeration; the mass of alumina added is 0.1% of the mass of the metal bonding powder to obtain a metal powder coating.
[0050] Example 3
[0051] A method for preparing a metal powder coating, the method comprising the following steps:
[0052] (1) Adding pigment and base powder into a bonding machine; the pigment is copper gold powder and pearlescent pigment, the particle size of the pigment is 30 to 100 μm, and the mass of the pigment is 8% of the mass of the base powder;
[0053] (2) nitrogen protective gas is introduced into the bonding machine, and the rotation speed of the low-speed stirring is set to 600 rpm; an interlayer is provided between the inner wall and the outer wall of the bonding kettle of the bonding machine, and heat source oil is introduced into the interlayer as a heat transfer medium, and the oil temperature of the heat source oil is maintained at 77-79° C., and the inner wall of the bonding kettle of the bonding machine is uniformly preheated, and the preheating bonding temperature is 77° C.;
[0054] (3) When the material temperature in the bonding machine reaches the preheating bonding temperature of 77° C. described in step (2), the bonding timing is started, and the bonding timing time is 180 seconds;
[0055] (4) After the bonding process is completed, the material is discharged into a cooling kettle connected to the bonding kettle. The outer wall of the cooling kettle is provided with an interlayer, and a stirring device is provided in the cooling kettle. Cold source water is introduced into the interlayer as a cooling medium. Under the action of stirring, the material discharged from the bonding kettle is fully contacted with the outer wall of the cooling kettle to achieve rapid cooling and obtain metal bonding powder;
[0056] (5) Take out the metal bonding powder obtained in step (4), sieve it and add alumina to improve fluidization and prevent agglomeration; the mass of alumina added is 0.3% of the mass of the metal bonding powder to obtain a metal powder coating.
[0057] The metal powder coatings prepared in Examples 1 to 3 were subjected to spraying experiments by a cyclone separation method and a high and low voltage method, and the spraying parameters were: a spraying voltage of 60 kV, an atomization starting pressure of 0.2 kPa, and a gun distance of 300 mm. The test results show that the visual effect of the metallic feel of the metal powders prepared in Examples 1 to 3 before and after cyclone separation is not much different, and the metallic feel is significantly enhanced with the increase of the pigment content in the metal powder coatings. At the same time, among the metal powder coatings prepared in Examples 1 to 3, the metal powder coating with a high pigment content (Example 3) has uniform powder discharge before and after cyclone separation under the same spraying conditions, and is not prone to gun clogging, indicating that in the metal powder coatings prepared by the method of the present invention, the pigment and the base powder form a good bonding effect.
[0058] The specific description above further illustrates the purpose, technical solutions and beneficial effects of the invention in detail. It should be understood that the above is only a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for preparing a metal powder coating, Features: The method steps are as follows: (1) Add pigment and primer into the bonding machine; The pigment is at least one of a metallic pigment and an imitation metallic pigment; the imitation metallic pigment is a pigment with a metallic luster; the particle size of the metallic pigment or the imitation metallic pigment is 30 to 100 μm; the medium particle size of the base material is 40 to 45 μm; The mass of the pigment is 3% to 8% of the mass of the base powder; (2) Introduce nitrogen protective gas into the bonding machine, set the low-speed stirring speed to 60 rpm to 600 rpm, and then evenly preheat the inner wall of the bonding kettle of the bonding machine. The preheating bonding temperature is (T g +10)℃~(T g +20)℃,T g is the glass transition temperature of the foundation powder; (3) When the material temperature in the bonding machine reaches the preheating bonding temperature, the bonding timing starts, and the bonding timing time is 180s to 600s; (4) After the bonding process is completed, the material is discharged into a cooling kettle connected to the bonding kettle for cooling to obtain metal bonding powder; (5) Take out the metal bonding powder, sieve it and add alumina, the mass of alumina added is 0.1% to 0.3% of the mass of the metal bonding powder, to obtain a metal powder coating.
2. A method for preparing a metal powder coating according to claim 1, Features: In step (1), the metallic pigment is copper gold powder; the imitation metallic pigment is pearlescent pigment; Taking the total mass of the base powder as 100%, the raw material components and their mass fractions are as follows: 70% polyester resin, 5% triglycidyl isocyanurate, 1% leveling agent, 0.3% benzoin, and 23.7% pigments and fillers; the pigments and fillers are a mixture of barium sulfate, red iron oxide, phthalocyanine blue and titanium dioxide.
3. A method for preparing a metal powder coating according to claim 1 or 2, Features: An interlayer is arranged between the inner wall and the outer wall of the bonding kettle of the bonding machine, and heat source water or heat source oil is introduced into the interlayer to uniformly preheat the interlayer of the bonding machine.
4. A method for preparing a metal powder coating according to claim 3, Features: In step (2), heat source water is introduced into the interlayer of the bonding kettle to uniformly preheat the interlayer of the bonding machine.
5. A method for preparing a metal powder coating according to claim 3, Features: In step (4), the cooling method is to set an interlayer on the outer wall of the cooling kettle, set a stirring device in the cooling kettle, and introduce cold source water or air flow into the interlayer as a cooling medium. Under the action of stirring, the discharge of the bonding kettle is brought into contact with the outer wall of the cooling kettle to achieve cooling.
Citation Information
Patent Citations
Bonded pearlescent powder coating and preparation method thereof
CN108102506A
Powder coating with bonding metal effect
CN108373765A
Anticorrosive powder coating for outdoor metal guardrails and preparation method thereof
CN110684443A
Weather-resistant optical energy storage metal powder coating and preparation method thereof
CN114276740A