Titanium alloy and preparation method thereof

By using titanium alloys of TiFeCrCoNi alloy powder and Cu powder, combined with atomization powdering and selective laser sintering technology, the problem of insufficient wear resistance of titanium alloy is solved, and titanium with high wear resistance and biocompatible is prepared. Alloy simplifies process flow and improves performance.

CN116790958BActive Publication Date: 2024-11-08JIANGXI UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310824160.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-06
Publication Date
2024-11-08
Estimated Expiration
2043-07-06

AI Technical Summary

Technical Problem

Due to insufficient wear resistance in biomedical implants, existing titanium alloys cause friction and wear to produce metal particles and debris, which endanger human health. The existing preparation methods and processes are complex, which limit the application of high wear-resistant biotitanium alloys.

Method used

The raw material powder of TiFeCrCoNi alloy powder and Cu powder is prepared by the master alloy preparation, atomization powder making and selective laser sintering process to prepare a titanium alloy with main phase FCC and enhanced phase HCP and Laves phase to achieve solid solution strengthening. , the combined effect of precipitation phase strengthening and fine crystal strengthening improves wear resistance and biocompatibility.

Benefits of technology

The prepared titanium alloy has excellent wear resistance and biocompatibility, low friction coefficient and small grains, which significantly improves the wear resistance and biocompatibility of biotitanium alloy, and has a simple process and reduces the production complexity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116790958B_ABST
    Figure CN116790958B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of titanium alloys, and specifically discloses a titanium alloy and a preparation method. The present invention provides a titanium alloy, which is prepared from raw material powders including TiFeCrCoNi alloy powder and Cu powder. According to the mass percentage of the raw material powder, the content of the TiFeCrCoNi alloy powder is 98.5-100%, and the content of the Cu powder is 0-1.5%, wherein the TiFeCrCoNi alloy powder includes the following components in atomic percentage: Fe: 17-23%, Cr: 17-23%, Co: 17-23%, Ni: 17-23%, and the balance is Ti. The preparation method of the titanium alloy provided by the present invention, combined with the atomization powder making process and the selective laser sintering process, can directly prepare a titanium alloy with excellent wear resistance and biocompatibility.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of titanium alloys, and in particular relates to a titanium alloy and a preparation method thereof. Background Art

[0002] Titanium and titanium alloys have become ideal materials for biomedical implants due to their excellent mechanical properties, biocompatibility, corrosion resistance and lower Young's modulus than natural bone. Their main applications include bone plates, bone nails, dental implants, cardiovascular stents, elbow joints, etc. However, titanium and its alloys often show poor wear resistance as supporting load-bearing implants, which will cause metal particles and debris to be generated during the friction and wear process after implantation in the human body, leading to the generation of "particle disease", which seriously endangers human health. Therefore, it is extremely important to develop new biomedical titanium alloys with high wear resistance.

[0003] The patent document with publication number CN115305385B discloses a low-cost, low-modulus, high-strength, high-wear-resistant bio-titanium alloy and its preparation method and application. The method melts the metal raw materials and then anneals them in a vacuum to obtain the low-cost, low-modulus, high-strength, high-wear-resistant bio-titanium alloy. However, when the metal raw materials are alloyed in the preparation method, the melting temperature is as high as 3400°C, and the alloy metal ingot needs to be turned over five times, which increases the complexity of the preparation process and limits the application of the high-wear-resistant bio-titanium alloy.

[0004] Therefore, there is an urgent need to provide a titanium alloy and a preparation method, which has a simple preparation process and can improve the wear resistance of the biological titanium alloy. Summary of the invention

[0005] The object of the present invention is to provide a titanium alloy and a preparation method thereof, which has a simple preparation process and can improve the wear resistance of the biological titanium alloy.

[0006] In a first aspect, the present invention provides a titanium alloy, which is prepared from raw material powders including TiFeCrCoNi alloy powder and Cu powder. Calculated by mass percentage of the raw material powders, the content of the TiFeCrCoNi alloy powder is 98.5-100%, and the content of the Cu powder is 0-1.5%, wherein the TiFeCrCoNi alloy powder includes the following components in atomic percentage: Fe: 17-23%, Cr: 17-23%, Co: 17-23%, Ni: 17-23%, and the balance is Ti.

[0007] Optionally, the titanium alloy includes a main phase FCC phase and a reinforcement phase, and the reinforcement phase includes a HCP phase and a Laves phase.

[0008] Optionally, the grain size of the titanium alloy is 0.1-10 μm.

[0009] Optionally, calculated by mass percentage of the raw material powder, the content of the TiFeCrCoNi alloy powder is 99.5-99.9%, and the content of the Cu powder is 0.1-0.5%, wherein the TiFeCrCoNi alloy powder includes the following components in atomic percentage: Fe: 19-21%, Cr: 19-21%, Co: 19-21%, Ni: 19-21%, and the balance is Ti.

[0010] Optionally, the grain size of the titanium alloy is 0.5-2.5 μm.

[0011] In a second aspect, the present invention provides a method for preparing the aforementioned titanium alloy, comprising the following steps:

[0012] (1) Preparation of raw material powder: TiFeCrCoNi alloy powder and Cu powder are weighed according to a ratio to obtain the raw material powder, wherein the preparation of the TiFeCrCoNi alloy powder comprises the following steps:

[0013] (1-1) Preparation of master alloy: weighing raw metals according to a ratio, smelting the raw metals, and preparing a master alloy;

[0014] (1-2) Atomization powder making: remelting the master alloy to obtain alloy liquid and then spraying powder making to obtain the TiFeCrCoNi alloy powder;

[0015] (2) The raw material powder is subjected to selective laser sintering to prepare a titanium alloy.

[0016] Optionally, in step (1-1), the raw metal is smelted at a temperature of 1600 to 1800° C., and the insulation time is 10 to 120 min.

[0017] Optionally, in step (1-2), the TiFeCrCoNi alloy powder prepared is a spherical powder, and the particle size of the powder is 15 to 35 μm.

[0018] Optionally, in step (1-2), the TiFeCrCoNi alloy powder prepared is an FCC phase.

[0019] Optionally, in step (2), the process parameters of the selective laser sintering are: laser spot size is 50-90 μm, laser scanning speed is 300-400 mm / s, laser power is 240-300 W, and scanning spacing is 0.06-0.08 mm.

[0020] In summary, the present invention has at least one of the following beneficial effects:

[0021] 1. A titanium alloy provided by the present invention is prepared from a raw material powder including a TiFeCrCoNi alloy powder. The five elements of the TiFeCrCoNi alloy powder form a high entropy alloy of a single supersaturated solid solution. The prepared titanium alloy includes a main phase FCC phase and a reinforcement phase HCP phase and a Laves phase, and has fine grains. At the same time, the comprehensive effects of solid solution strengthening, precipitation phase strengthening and fine grain strengthening are achieved. Therefore, the titanium alloy has excellent wear resistance and biocompatibility. The friction coefficient of the titanium alloy is below 0.2, and preferably below 0.16.

[0022] 2. The titanium alloy provided by the present invention utilizes TiFeCrCoNi alloy powder and Cu powder in a specific ratio and utilizes the synergistic effect between alloy elements to further improve the wear resistance and biocompatibility of the titanium alloy.

[0023] 3. The present invention provides a method for preparing a titanium alloy, which combines an atomization powder making process and a selective laser sintering process, and uses a raw material powder including a specific proportion of TiFeCrCoNi alloy powder and Cu powder for selective laser sintering. The process is simple and can directly prepare a biological titanium alloy with excellent wear resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a scanning electron microscope image of the TiFeCrCoNi alloy powder prepared in Example 1;

[0025] Figure 2 XRD pattern of the TiFeCrCoNi alloy powder prepared in Example 1;

[0026] Figure 3 XRD pattern of the titanium alloy prepared in Example 1;

[0027] Figure 4 This is a SEM image of the titanium alloy prepared in Example 1;

[0028] Figure 5 This is the friction performance test curve of the titanium alloy prepared in Example 1;

[0029] Figure 6 This is a wear scar diagram of the friction performance test of the titanium alloy prepared in Example 1;

[0030] Figure 7 This is an inverted fluorescence microscope image of the biocompatibility of the titanium alloy prepared in Example 1;

[0031] Figure 8 This is an inverted fluorescence microscope image of the biocompatibility of the titanium alloy prepared in Example 2;

[0032] Fig. 9 This is an inverted fluorescence microscope image of the biocompatibility of the titanium alloy prepared in Example 3;

[0033] Fig.10 An inverted fluorescence microscope image of the biocompatibility of the titanium alloy prepared in Example 4;

[0034] Fig.11 This is the friction performance test curve of pure titanium prepared in Comparative Example 1;

[0035] Fig.12 This is the wear scar image of the friction performance test of pure titanium prepared in Comparative Example 1;

[0036] Fig.13 This is the friction performance test curve of the titanium alloy prepared in Comparative Example 2;

[0037] Fig.14 This is an inverted fluorescence microscope image of the biocompatibility of the titanium alloy prepared in Comparative Example 2. DETAILED DESCRIPTION

[0038] The present invention provides a titanium alloy and a preparation method. To make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0039] The present invention provides a titanium alloy, which is prepared from raw material powders including TiFeCrCoNi alloy powder and Cu powder. According to the mass percentage of the raw material powder, the content of TiFeCrCoNi alloy powder is 98.5-100%, and the content of Cu powder is 0-1.5%, wherein the TiFeCrCoNi alloy powder includes the following components in atomic percentage: Fe: 17-23%, Cr: 17-23%, Co: 17-23%, Ni: 17-23%, and the balance is Ti. The titanium alloy prepared by using the TiFeCrCoNi alloy powder and Cu powder in a specific ratio has excellent wear resistance and biocompatibility, a friction coefficient of less than 0.2, and an absorbance of 0.65-0.71.

[0040] In some embodiments of the present invention, the content of TiFeCrCoNi alloy powder is 99.5-99.9%, and the content of Cu powder is 0.1-0.5%. TiFeCrCoNi alloy powder includes the following components in atomic percentage: Fe: 19-21%, Cr: 19-21%, Co: 19-21%, Ni: 19-21%, and the balance is Ti. Preferably, Ti, Fe, Cr, Co, and Ni are in equal atomic ratios. The titanium alloy prepared by using TiFeCrCoNi alloy powder and Cu powder within this range has better wear resistance and biocompatibility, with a friction coefficient of less than 0.11 and an absorbance of more than 0.71.

[0041] In some embodiments of the invention, the titanium alloy includes a main phase FCC phase and a reinforcement phase, and the reinforcement phase includes an HCP phase and a Laves phase. The main phase FCC (face-centered cubic) phase is a supersaturated solid solution, and the HCP (hexagonal) phase and the Laves phase are dispersed in the main phase FCC, which plays the role of solid solution strengthening and precipitation phase strengthening, and can improve the wear resistance of the titanium alloy.

[0042] In some embodiments of the invention, the grain size of the titanium alloy is 0.1-10 μm, preferably 0.5-5.0 μm, and more preferably 0.5-2.5 μm. The fine grain structure of the titanium alloy can play a role of fine grain strengthening, further improving the wear resistance of the titanium alloy.

[0043] The present invention provides a method for preparing a titanium alloy, comprising the following steps:

[0044] (1) Preparation of raw material powder: TiFeCrCoNi alloy powder and Cu powder are weighed according to a ratio to obtain raw material powder, wherein the preparation of TiFeCrCoNi alloy powder includes the following steps:

[0045] (1-1) Preparation of master alloy: weighing raw metals according to the ratio, smelting the raw metals, and preparing the master alloy;

[0046] (1-2) Atomization powder making: The master alloy is remelted to obtain alloy liquid, and then spray powder making is performed to obtain TiFeCrCoNi alloy powder;

[0047] (2) The raw material powder is subjected to selective laser sintering to prepare a titanium alloy.

[0048] In some embodiments of the present invention, in step (1-1), the raw metal is smelted at a temperature of 1600-1800°C and the holding time is 10-120 minutes. Preferably, the smelting temperature is 1700-1800°C and the holding time is 40-80 minutes. The above-mentioned smelting temperature and holding time are conducive to obtaining a master alloy with uniform composition.

[0049] In some embodiments of the present invention, in step (1-2), the TiFeCrCoNi alloy powder prepared is spherical powder, and the particle size of the powder is 15 to 35 μm. The use of alloy powders in the above particle size range is conducive to improving the fluidity and formability of the alloy powder in the subsequent selective sintering process.

[0050] In some embodiments of the present invention, in step (1-2), the TiFeCrCoNi alloy powder prepared is in FCC phase. Using FCC phase high entropy titanium alloy powder is conducive to preparing high entropy titanium alloy by selective sintering.

[0051] In one embodiment of the present invention, in step (2), the process parameters of selective laser sintering are: laser spot size is 50-90 μm, preferably 65-75 μm, laser scanning speed is 300-400 mm / s, preferably 330-370 mm / s, laser power is 240-300 W, preferably 250-280 W, and scanning spacing is 0.06-0.08 mm. By using the process parameters of selective laser sintering within the above range, a titanium alloy with excellent wear resistance and biocompatibility can be prepared.

[0052] The present invention is described in detail below with reference to specific embodiments and comparative examples.

[0053] Example 1

[0054] This embodiment provides a method for preparing a titanium alloy, comprising the following steps:

[0055] (1) Preparation of raw material powder: TiFeCrCoNi alloy powder is weighed according to the ratio to obtain raw material powder, wherein the preparation of TiFeCrCoNi alloy powder includes the following steps:

[0056] (1-1) Preparation of master alloy: The ingredients are prepared according to the atomic percentage of Ti: 20at.%, Fe: 20at.%, Cr: 20at.%, Co: 20at.%, and Ni: 20at.%, and the metal raw materials are pure titanium, pure iron, pure chromium, pure cobalt, and pure nickel. The purity of the metal raw materials is 99.9%. The metal raw materials are added to the induction melting furnace and vacuumed to 9×10 -3 Pa, heated to 1750 ° C and kept warm for 50 minutes, and then refined. After the refining is completed, the alloy liquid is poured and solidified to prepare the mother alloy.

[0057] (1-2) Atomization powder making: The master alloy is crushed into alloy blocks, and then the alloy blocks are added to the crucible of the atomization powder making equipment. The alloy blocks are heated and remelted by vacuum induction melting to obtain alloy liquid. The alloy liquid is purged with high-purity argon gas, and the alloy liquid is sprayed to obtain TiFeCrCoNi alloy powder. The specific process parameters of atomization powder making are: argon gas flow pressure of 3.3MPa, gas flow velocity of 320m / s.

[0058] Figure 1 This is a SEM image of the TiFeCrCoNi alloy powder prepared in Example 1. The prepared TiFeCrCoNi alloy powder is spherical powder with a particle size of 15 to 35 μm. The powder has high sphericity and a small amount of symbiotic satellite spherical powder.

[0059] Figure 2 The XRD pattern of the TiFeCrCoNi alloy powder prepared in Example 1 is shown in FIG. Figure 2 It can be seen that the TiFeCrCoNi alloy powder is a single FCC phase, and the FCC phase is a highly supersaturated solid solution, which is a typical feature of high entropy alloy (HEA). It can be seen that the prepared TiFeCrCoNi alloy powder is a high entropy alloy powder.

[0060] (2) The raw material powder is subjected to selective laser sintering to prepare a titanium alloy. Specifically, the raw material powder is placed in the feeding bin of the selective laser sintering system, the laser is a CO2 laser, the laser spot is set to 70μm, the scanning spacing is set to 0.07mm, the laser power is set to 260W, and the laser scanning speed is set to 350mm / s. The raw material powder is scanned and sintered layer by layer. After each laser scan completes a layer, the printing work plane is lowered, the next layer of raw material powder is laid on its top surface, and then a new layer is laser scanned. The above process is repeated to finally prepare a titanium alloy.

[0061] Figure 3 The XRD pattern of the titanium alloy prepared in Example 1 is shown in FIG. Figure 3 It can be seen that in addition to the main phase FCC phase, the titanium alloy also has a small amount of reinforcement phase HCP phase and Laves phase. It can be seen that the prepared titanium alloy also has the typical characteristics of high entropy alloys.

[0062] Figure 4 This is the SEM image of the titanium alloy prepared in Example 1. Figure 4 It can be seen that the prepared titanium alloy has fine and uniform grains, with a grain size of 0.5 to 2.5 μm.

[0063] Figure 5 The friction test performance test curve of the titanium alloy prepared in Example 1 is obtained by using the reciprocating friction and wear method. Figure 5 It can be seen that the friction coefficient of titanium alloy is very small, only 0.14, and with the increase of friction time, the friction coefficient hardly changes, which is attributed to the combined effect of high solid solution strengthening, precipitation phase strengthening and fine grain strengthening of high entropy alloy.

[0064] Figure 6 This is the wear scar diagram of the friction test of the titanium alloy of Example 1. Figure 6 It can be seen that the wear scar of titanium alloy is shallow, the wear scar width is 220μm, and the wear amount is very low, indicating that the wear resistance of titanium alloy is excellent.

[0065] Figure 7 The biological cytotoxicity test of the titanium alloy prepared in Example 1 was conducted by inverted fluorescence microscopy. The live and dead cells cultured on the titanium alloy surface of Example 1 for 7 days were analyzed. Figure 7It can be seen that after 7 days of culture, the cells on the surface of the titanium alloy have good cell activity and a large number of cells. When a cell counting reagent (CCK-8) is added and the absorbance is measured at 450nm, the value is 0.70, indicating that a large number of cells survive and the titanium alloy has excellent biocompatibility.

[0066] Example 2

[0067] The difference between Example 2 and Example 1 is that in step (1-1), the master alloy is prepared by mixing the ingredients according to the atomic percentage of Ti: 24at.%, Fe: 19at.%, Cr: 19at.%, Co: 19at.%, and Ni: 19at.%, and the remaining preparation steps are the same as those in Example 1 to prepare a titanium alloy.

[0068] XRD was used to perform phase analysis on the titanium alloy prepared in Example 2, and it was found that the titanium alloy prepared in Example 2 was mainly composed of FCC phase, a small amount of α-Ti phase, and strengthening phases HCP phase and Laves phase, and also had the characteristics of a typical high entropy alloy. The grain size of the titanium alloy prepared in Example 2 was 3.0 to 8.6 μm. Compared with Example 1, the grain size of the titanium alloy in Example 2 was increased. The wear resistance of the titanium alloy in Example 2 was tested by the same reciprocating friction and wear method as in Example 1, and the friction coefficient of the titanium alloy was measured to be 0.20. It can be seen that the wear resistance of the titanium alloy in Example 2 is reduced compared with the wear resistance of the titanium alloy in Example 1.

[0069] The biological cytotoxicity of the titanium alloy prepared in Example 2 was tested using the same method as in Example 1. Figure 8 This is an inverted fluorescence microscope image of the titanium alloy prepared in Example 2. Figure 8 It can be seen that the cells on the surface of the titanium alloy of Example 2 have good cell activity and a large number of cells after 7 days of culture. When a cell counting reagent (CCK-8) is added and the absorbance is measured at 450nm, the value is 0.67, indicating that a large number of surviving cells and the titanium alloy has high biocompatibility. It can be seen that the biocompatibility of the titanium alloy of Example 2 is lower than that of the titanium alloy of Example 1.

[0070] Example 3

[0071] The difference between Example 3 and Example 1 is that in step (1), the raw powder is prepared by weighing TiFeCrCoNi alloy powder and Cu powder (commercially available, with a purity of 99.9% and a particle size of 15 to 35 μm) according to a ratio, and mixing them to obtain the raw powder. According to the mass percentage of the raw powder, the content of TiFeCrCoNi alloy powder is 99.5%, and the content of Cu powder is 0.5%. The remaining preparation steps are the same as in Example 1 to prepare a titanium alloy.

[0072] XRD was used to perform phase analysis on the titanium alloy prepared in Example 3, and it was found that the main phase of the titanium alloy prepared in Example 3 was FCC phase, and also included a small amount of reinforcing phase HCP phase and Laves phase, which also had the characteristics of a typical high entropy alloy. The grain size of the titanium alloy prepared in Example 3 was 0.5-2.0 μm. Compared with Example 1, the grain size of the titanium alloy in Example 3 was reduced. The wear resistance of the titanium alloy in Example 3 was tested by the same reciprocating friction and wear method as in Example 1, and the friction coefficient of the titanium alloy was measured to be 0.11, and the friction coefficient hardly changed with the increase of friction time. It can be seen that the wear resistance of the titanium alloy in Example 3 is improved compared with the wear resistance of the titanium alloy in Example 1.

[0073] The biological cytotoxicity of the titanium alloy prepared in Example 3 was tested using the same method as in Example 1. Fig. 9 This is an inverted fluorescence microscope image of the titanium alloy prepared in Example 3. Fig. 9 It can be seen that the cells on the surface of the titanium alloy of Example 3 have good cell activity and a large number of cells after 7 days of culture. When a cell counting reagent (CCK-8) is added and the absorbance is measured at 450nm, the value is 0.71, indicating that a large number of surviving cells and the titanium alloy has high biocompatibility. It can be seen that the biocompatibility of the titanium alloy of Example 3 is slightly better than that of the titanium alloy of Example 1.

[0074] Example 4

[0075] The difference between Example 4 and Example 1 is that in step (1), the raw powder is prepared by weighing TiFeCrCoNi alloy powder and Cu powder (commercially available, with a purity of 99.9% and a particle size of 15 to 35 μm) according to a ratio, and mixing them to obtain the raw powder. According to the mass percentage of the raw powder, the content of TiFeCrCoNi alloy powder is 99%, and the content of Cu powder is 1%. The remaining preparation steps are the same as in Example 1 to prepare a titanium alloy.

[0076] XRD was used to perform phase analysis on the titanium alloy prepared in Example 4, and it was found that the main phase of the titanium alloy prepared in Example 4 was FCC phase, and also included a small amount of reinforcing phase HCP phase and Laves phase, which also had the characteristics of a typical high entropy alloy. The grain size of the titanium alloy prepared in Example 4 was 1.5 to 5.0 μm. Compared with Example 1, the grain size of the titanium alloy in Example 4 increased. The wear resistance of the titanium alloy in Example 4 was tested by the same reciprocating friction and wear method as in Example 1, and the friction coefficient of the titanium alloy was measured to be 0.16. It can be seen that the wear resistance of the titanium alloy in Example 4 is reduced compared with the wear resistance of the titanium alloy in Example 1.

[0077] The biological cytotoxicity of the titanium alloy prepared in Example 4 was tested using the same method as in Example 1. Fig.10 This is an inverted fluorescence microscope image of the titanium alloy prepared in Example 4. Fig.10 It can be seen that the cells on the surface of the titanium alloy of Example 4 have good cell activity and a large number of cells after 7 days of culture. When a cell counting reagent (CCK-8) is added and the absorbance is measured at 450 nm, the value is 0.65, indicating that a large number of surviving cells and the titanium alloy has high biocompatibility. It can be seen that the biocompatibility of the titanium alloy of Example 4 is lower than that of the titanium alloy of Example 1.

[0078] Comparative Example 1

[0079] Comparative Example 1 provides a method for preparing pure titanium, comprising the following steps of selectively laser sintering titanium powder (commercially available, with a purity of 99.9% and a particle size of 15 to 35 μm) to prepare pure titanium. Specifically, the raw material powder is placed in a selective laser sintering feed bin, a CO2 laser is used as the laser, the laser spot is set to 70 μm, the scanning spacing is set to 0.07 mm, the laser power is set to 260 W, the laser scanning speed is set to 350 mm / s, and the raw material powder is scanned and sintered layer by layer. After each laser scan completes a layer, the printing work plane is lowered, and the next layer of raw material powder is laid on its top surface, and then a new layer is laser scanned. Repeat the above process in this way, and pure titanium is finally prepared.

[0080] The wear resistance of the pure titanium in Comparative Example 1 was tested using the same reciprocating friction and wear method as in Example 1. Fig.11 The friction test performance test curve of pure titanium prepared in Comparative Example 1 is shown in FIG. Fig.11 It can be seen that the friction coefficient of the pure titanium prepared in Comparative Example 1 is between 0.4 and 0.55. It can be seen that the wear resistance of the pure titanium in Comparative Example 1 is significantly inferior to that of the titanium alloy prepared in Example 1.

[0081] Fig.12 This is the wear scar diagram of the friction test of pure titanium in comparative example 1. Fig.12 It can be seen that compared with the titanium alloy of Example 1, the wear scar of the pure titanium prepared in Comparative Example 1 is deeper, the wear scar width is 750 μm, and the wear amount is significantly increased.

[0082] Comparative Example 2

[0083] The difference between Comparative Example 2 and Example 1 is that, in step (1), the raw powder is prepared by weighing TiFeCrCoNi alloy powder and Mn powder (commercially available, with a purity of 99.9% and a particle size of 15 to 35 μm) according to a ratio, and mixing them to obtain the raw powder. According to the mass percentage of the raw powder, the content of TiFeCrCoNi alloy powder is 99%, and the content of Mn powder is 1%. The remaining preparation steps are the same as in Example 1 to prepare a titanium alloy.

[0084] The titanium alloy prepared in Comparative Example 2 was analyzed by XRD, and the main phase of the titanium alloy prepared in Comparative Example 2 was FCC phase, and a small amount of HCP phase and Laves phase were also included, which also had the characteristics of a typical high entropy alloy. The grain size of the titanium alloy prepared in Comparative Example 2 was 1.5-5.5 μm, and the grain size of the titanium alloy in Comparative Example 2 was increased compared with Example 1.

[0085] The wear resistance of the titanium alloy of Comparative Example 2 was tested by the same reciprocating friction and wear method as in Example 1. Fig.13 The friction test performance test curve of the titanium alloy prepared in Comparative Example 2 is shown in FIG. Fig.13 It can be seen that the friction coefficient of the titanium alloy prepared in Comparative Example 2 is between 0.16 and 0.18. It can be seen that the wear resistance of Comparative Example 2 is lower than that of the titanium alloy prepared in Example 1.

[0086] The biological cytotoxicity of the titanium alloy prepared in Comparative Example 2 was tested using the same method as in Example 1. Fig.14 This is an inverted fluorescence microscope image of the titanium alloy prepared in Comparative Example 2. Fig.14 It can be seen that the cells on the surface of the titanium alloy of Example 4 have good cell activity and a large number of cells after 7 days of culture. When a cell counting reagent (CCK-8) is added and the absorbance is measured at 450 nm, the value is 0.62. It can be seen that the biocompatibility of the titanium alloy of Comparative Example 2 is significantly inferior to that of the titanium alloy of Example 1.

[0087] The above are all preferred embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Therefore, any equivalent changes made based on the structure, shape, and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A titanium alloy, characterized in that: The titanium alloy is prepared from raw powders consisting of TiFeCrCoNi alloy powder and Cu powder. Calculated by mass percentage of the raw powders, the content of the TiFeCrCoNi alloy powder is 99.5-99.9%, and the content of the Cu powder is 0.1-0.5%. The TiFeCrCoNi alloy powder has the following components in atomic percentage: Fe: 19-21%, Cr: 19-21%, Co: 19-21%, Ni: 19-21%, and the balance is Ti.

2. A titanium alloy according to claim 1, characterized in that: The titanium alloy includes a main phase FCC phase and a reinforcement phase, and the reinforcement phase includes a HCP phase and a Laves phase.

3. A titanium alloy according to claim 1, characterized in that: The grain size of the titanium alloy is 0.1-10 μm.

4. A titanium alloy according to claim 1, characterized in that: The grain size of the titanium alloy is 0.5-2.5 μm.

5. A method for preparing the titanium alloy according to any one of claims 1 to 4, characterized in that: The following steps are involved: (1) Preparation of raw material powder: TiFeCrCoNi alloy powder and Cu powder are weighed according to a ratio to obtain the raw material powder, wherein the preparation of the TiFeCrCoNi alloy powder comprises the following steps: (1-1) Preparation of master alloy: weighing raw metals according to a ratio, smelting the raw metals, and preparing a master alloy; (1-2) Atomization powder making: remelting the master alloy to obtain alloy liquid and then spraying powder making to obtain the TiFeCrCoNi alloy powder; (2) The raw material powder is subjected to selective laser sintering to prepare a titanium alloy.

6. The method for preparing a titanium alloy according to claim 5, characterized in that: In step (1-1), the raw metal is smelted at a temperature of 1600-1800° C. and the holding time is 10-120 min.

7. The method for preparing a titanium alloy according to claim 5, characterized in that: In step (1-2), the TiFeCrCoNi alloy powder prepared is a spherical powder with a particle size of 15 to 35 μm.

8. The method for preparing a titanium alloy according to claim 5, characterized in that: In step (1-2), the TiFeCrCoNi alloy powder prepared is an FCC phase.

9. The method for preparing a titanium alloy according to claim 5, characterized in that: In step (2), the process parameters of the selective laser sintering are: laser spot size is 50-90 μm, laser scanning speed is 300-400 mm / s, laser power is 240-300 W, and scanning spacing is 0.06-0.08 mm.