A cold-formed high-corrosion-resistant color-coated steel plate and its production method

Through chemical composition optimization and process improvement, the problem of short service life of cold-formed high-corrosion-resistant color-coated sheets in complex corrosive environments has been solved, the acid and alkali resistance and processing performance of the coating have been improved, and the service life of the building has been extended. .

CN116790973BActive Publication Date: 2024-10-29МААНЬШАНЬ АЙРОН ЭНД СТИЛ КО ЛТД
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310316676.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-29
Estimated Expiration
2043-03-29

AI Technical Summary

Technical Problem

The existing cold-formed high-corrosion-resistant color-coated sheets have a short service life in complex corrosive environments and are prone to coating cracking and low acid and alkali corrosion resistance, which affects industrial production and maintenance costs.

Method used

Adopt highly corrosion-resistant color-coated steel plates with optimized chemical composition, including coating components Mg, Si, Al, Zn, etc., through hot-dip galvanized aluminum-magnesium substrate process, multi-terminated hydroxyl polyester resin, anti-corrosion additives and phosphate anti-rust pigments and fillers , optimize the coating structure and process flow, improve the cross-linking density and compactness of the coating, and enhance the resistance to acid and alkali media.

Benefits of technology

It significantly improves the service life of high-corrosion-resistant color-coated boards in complex corrosive environments, enhances the coating's resistance to oxidizing media corrosion and penetration, meets complex cold forming processing requirements, and extends the service life of buildings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a cold-formed high corrosion-resistant color-coated steel plate and a production method thereof, belonging to the technical field of metal iron-based surface coating. The invention comprises the following chemical components in weight percentage: C: 0.01% to 0.10%, Si: 0.08% to 0.10%, Mn: 0.40% to 0.50%, P: 0.030% to 0.035%, S: 0.025% to 0.035%, and the rest is Fe and other inevitable impurities; wherein the double-sided coating weight of the high corrosion-resistant color-coated steel plate is ≥100g / m 2 , the coating composition includes the following chemical components in weight percentage: Mg: 1% to 2%, Si: 1% to 2%, Al: 50% to 55%, and the rest is Zn. The present invention can produce high corrosion resistant color coated plates that meet the requirements of complex cold forming processing, effectively solve the problems of cracking of complex cold forming coatings, low acid and alkali corrosion resistance of coatings, and improve the service life of high corrosion resistant color coated plates in complex corrosive environments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal iron-based surface coating, and more specifically, relates to a cold-formed high-corrosion-resistant color-coated steel plate and a production method thereof. Background Art

[0002] Color-coated panels, with their advantages of beauty, energy saving, and easy and efficient construction, have been widely used in building enclosure systems in large venues, industrial plants, transportation and other fields, with a service life of more than 20 years. However, in industries such as animal husbandry, food processing, non-ferrous smelting, chemical production, ceramic cement, etc., a large amount of acidic media containing chloride ions, sulfides, and nitrides, alkaline corrosive media containing ammonia and basic carbonates are generated during industrial activities, and complex corrosive atmospheres in the form of high temperature, high humidity, and dust cause serious corrosion to the building enclosure structure of the factory. The above-mentioned industries use ordinary color-coated panels as the building enclosure structure of the factory, and their service life is usually only 3-5 years.

[0003] In addition, the high corrosion-resistant coating is prone to deformation, cracking, coating thinning and other problems during cold forming, resulting in a reduction in the service life of the product. This not only seriously affects normal industrial production, but also increases the cost of building maintenance and replacement. Therefore, it is urgent to design a cold-formed high corrosion-resistant color-coated steel plate and its production method, which can produce high corrosion-resistant color-coated plates that meet the requirements of complex cold forming processing, effectively solve the problems of complex cold forming coating cracking, low acid and alkali resistance of the coating, and improve the service life of high corrosion-resistant color-coated plates in complex corrosive environments.

[0004] After searching, relevant patent documents on the technology of high corrosion-resistant color-coated plates have been disclosed, such as the Chinese patent "High corrosion-resistant deep-drawn color-coated plates for outdoor household appliances and preparation methods thereof" (publication number CN114535036A) discloses a household appliance deep-drawn color-coated plate; the patent "An environmentally friendly PCM color pre-coated plate and preparation method thereof" (CN113954458A) discloses a multi-layer composite membrane structural steel plate; the patent "A corrosion-resistant composite color-coated plate and preparation method thereof" (publication number CN112795279A) discloses a non-environmentally friendly color-coated plate with pure zinc coating. However, the above patents cannot solve the problems of cracking of complex cold-formed coatings and low corrosion resistance of coatings such as acid and alkali resistance. Summary of the invention

[0005] 1. Problems to be solved

[0006] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, one purpose of the present invention is to provide a cold-formed high-corrosion-resistant color-coated steel plate and a production method thereof, which can produce a high-corrosion-resistant color-coated plate that meets the requirements of complex cold-formed processing, effectively solve the problems of cracking of complex cold-formed coatings, low acid and alkali corrosion resistance of coatings, and improve the service life of high-corrosion-resistant color-coated plates in complex corrosive environments.

[0007] 2. Technical solution

[0008] To solve the above problems, the present invention adopts the following technical solutions.

[0009] A cold-formed high-corrosion-resistant color-coated steel plate of the present invention comprises the following chemical components in weight percentage: C: 0.01% to 0.10%, Si: 0.08% to 0.10%, Mn: 0.40% to 0.50%, P: 0.030% to 0.035%, S: 0.025% to 0.035%, and the rest is Fe and other inevitable impurities;

[0010] The double-sided coating weight of high corrosion resistant color-coated steel sheet is ≥100g / m 2 The coating composition includes the following chemical components in weight percentage: Mg: 1% to 2%, Si: 1% to 2%, Al: 50% to 55%, and the rest is Zn.

[0011] As a further improvement of the present invention, the following process flow is included: hot-dip galvanized aluminum-magnesium substrate → cleaning → passivation → drying → initial coating of front primer / back primer → curing → water cooling → fine coating of front topcoat / back topcoat → curing → water cooling → inspection → coiling, wherein in the hot-dip galvanized aluminum-magnesium substrate process step, the temperature of the strip entering the zinc pot is controlled to be within the range of 575±5°C, and the temperature of the zinc pot is controlled to be within the range of 585±5°C.

[0012] As a further improvement of the present invention, in the process steps of hot-dip galvanizing aluminum-magnesium substrate, the distance between the front air knife, the rear air knife and the strip steel is controlled to be 2.0 cm to 2.5 cm, and the opening range of the cooling fan is 20% to 30%, and the air flow rate is 18000m 3 / h~22000m 3 / h.

[0013] As a further improvement of the present invention, the ratio of the polyester resin with multiple terminal hydroxyl groups to the linear polyester resin in the topcoat is 1:4 to 1:2, and the content of the anti-corrosion additive in the topcoat is 15% to 20%.

[0014] As a further improvement of the present invention, the proportion of nano-scale pigments and fillers in the topcoat coating exceeds 80%.

[0015] As a further improvement of the present invention, the topcoat contains a fluoride as a high-temperature melting sealing material, and the ratio of the light-colored coating resin to the pigment filler in the topcoat is controlled to be ≤0.8.

[0016] As a further improvement of the present invention, in the cleaning process steps, the strip steel is subjected to two alkali washes, the alkali solution concentration is 0.5% to 1.5%, and the alkali solution temperature is 45°C to 60°C; the steel plate after alkali washing is then subjected to three water washes, the water washing temperature is 40°C to 65°C, wherein the last water wash uses desalted water, and the conductivity of the desalted water is ≤0.2ms / cm.

[0017] As a further improvement of the present invention, in the passivation process step, a layer of water-soluble organic polymer containing titanic acid and phosphate is coated on the surface of the strip, and after drying in a curing furnace at 80°C to 100°C, a passivation layer with a film thickness of 0.5μm to 1.0μm is formed.

[0018] As a further improvement of the present invention, the passivated strip enters into a roller coating room for initial primer coating, the primer coating viscosity is 8s to 20s, and the primer coating is applied to the surface of the strip by continuous two-roll reverse coating; then the strip enters into a curing furnace for drying, and the curing time in the curing furnace is controlled to be ≤35s, and the curing PMT temperature is ≤232°C. After the strip exits the curing furnace, it enters into a water quenching tank, and then is dried by cold air, and the thickness of the primer film formed is 5μm to 15μm.

[0019] As a further improvement of the present invention, when the steel strip after primer coating is applied is topcoated, the topcoat coating has a viscosity of 15s to 30s, and a continuous three-roll reverse coating method is used to apply the topcoat coating on the surface of the strip, and then the strip enters a curing furnace for drying, and the curing time is controlled to be ≤33s, and the curing PMT temperature is ≤241°C; after the strip exits the curing furnace, it enters a water quenching tank, and then is dried by cold air to form a topcoat dry film thickness of 15μm to 25μm.

[0020] 3. Beneficial effects

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] (1) The present invention provides a method for producing cold-formed highly corrosion-resistant color-coated steel plates. To solve the problems of cracking of complex cold-formed coatings and low acid and alkali corrosion resistance of the coatings, the process design and optimization of the steel plates and coating components are used to modify the coating pigments and fillers to improve the chemical inertness of the coatings in acidic and alkaline environments. The cross-linking density and compactness of the coatings are improved by optimizing the design of the coating system and the coating structure as well as optimizing the coating curing process, thereby improving the corrosion resistance and penetration of the coatings to oxidative media, and manufacturing highly corrosion-resistant and environmentally friendly color-coated plates that meet the requirements of complex cold-formed processing.

[0023] (2) The present invention provides a method for producing cold-formed high-corrosion-resistant color-coated steel sheets, which strengthens the cooling control of the strip steel when it leaves the zinc pot, increases the opening and air volume of the cooling fan, accelerates the cooling of the zinc liquid, and inhibits the growth of zinc flowers, thereby reducing the size of the zinc flowers; adjusts the position and angle of the air knife, reduces the distance between the air knife and the strip steel, and can more accurately control the surface coating and reduce the fluctuation of the zinc layer.

[0024] (3) A production method of a cold-formed high-corrosion-resistant color-coated steel sheet of the present invention, the topcoat uses a polyester resin with multiple terminal hydroxyl groups, and the linear polyester resin is grafted and strengthened at a ratio of 1:4 to 1:2, the number of hydroxyl groups is increased by 10%, the cross-linking density of the film-forming material is increased, and the solvent resistance of the system is improved, and the corrosion resistance of the paint film to corrosive media is effectively improved; at the same time, 15% to 20% of an anti-corrosion additive is added to the film-forming material to further strengthen the chemical resistance to oxidizing media and acidic and alkaline media. .

[0025] (4) The present invention provides a method for producing cold-formed highly corrosion-resistant color-coated steel plates, wherein the primer adopts a polyurethane coating system with high corrosion resistance. By optimizing the cross-linking agent, the active substituent groups of the coating are fully cross-linked during the curing process, and the molecular space is tightly arranged, which effectively prevents the acid-base medium molecules from penetrating and diffusing into the interior of the paint film.

[0026] (5) The present invention provides a method for producing a cold-formed high-corrosion-resistant color-coated steel sheet. The primer uses a phosphate anti-rust pigment filler. The phosphate releases phosphate during the slow hydrolysis process. The phosphate ions combine with metal ions to form a dense and strong complex protective film with strong adhesion, which protects the metal surface, improves the corrosion resistance of the color-coated sheet, and realizes chromium-free and environmentally friendly DETAILED DESCRIPTION

[0027] In order to further understand the content of the present invention, a detailed description is given in conjunction with the present invention.

[0028] The specific implementation methods of the present invention are further explained in detail below through the description of implementation examples.

[0029] Example 1

[0030] A cold-formed high corrosion-resistant color-coated steel sheet in this embodiment includes the following chemical components in weight percentage: C: 0.01% to 0.10%, Si: 0.08% to 0.10%, Mn: 0.40% to 0.50%, P: 0.030% to 0.035%, S: 0.025% to 0.035%, and the rest is Fe and other inevitable impurities. Specifically, the cold-formed high corrosion-resistant color-coated steel sheet in this embodiment includes the following chemical components in weight percentage: C: 0.01%, Si: 0.08%, Mn: 0.50%, P: 0.035%, S: 0.035%, and the rest is Fe and other inevitable impurities

[0031] The double-sided coating weight of the high corrosion-resistant color-coated steel plate in this embodiment is ≥100g / m 2 , wherein the coating composition includes the following chemical components in weight percentage: Mg: 1% to 2%, Si: 1% to 2%, Al: 50% to 55%, and the rest is Zn. In this embodiment, Si and Mg are easily combined to form Mg2Si phase, and the coating is easily dissolved and produced Mg in the initial stage of corrosion. 2+ Favorable conditions are created for the formation of insoluble and dense metal hydroxides. In addition, the formation of Mg2Si phase can effectively inhibit the violent reaction of Si and Al elements between the coating and the substrate, and prevent the thickness of the inhibition layer from increasing; when the Si element exceeds 2%, the single free Si phase in the coating increases, which deteriorates the corrosion resistance of the coating; when the Mg element exceeds 2%, the surface quality of the coating decreases, the production difficulty increases, and the subsequent color coating process is adversely affected. Specifically, the coating composition in this embodiment includes the following chemical components in weight percentage: Mg: 1.2%, Si: 1%, Al: 50%, and the rest is Zn.

[0032] A production method of cold-formed high corrosion-resistant color-coated steel plate in this embodiment adopts a two-coating and two-baking method, including the following process flow: hot-dip galvanized aluminum-magnesium substrate → cleaning → passivation → drying → initial coating of front primer / back primer → curing → water cooling → fine coating of front topcoat / back topcoat → curing → water cooling → inspection → coiling, wherein the temperature of the hot-dip galvanized aluminum-magnesium substrate process step is controlled within the range of 575±5℃ when the strip enters the zinc pot, and the temperature of the zinc pot is controlled within the range of 585±5℃. Furthermore, the distance between the front air knife, the rear air knife and the strip is controlled to be 2.0cm~2.5cm, and the opening range of the cooling fan is 20%~30%, and the air flow rate is 18000m 3 / h~22000m 3 / h, strengthen the cooling control of the strip when it leaves the zinc pot, increase the opening and air volume of the cooling fan, accelerate the cooling of the zinc liquid, inhibit the growth of zinc flowers, and thus reduce the size of the zinc flowers; adjust the position and angle of the air knife, reduce the distance between the air knife and the strip, and more accurately control the surface coating and reduce the fluctuation of the zinc layer. Specifically, in this embodiment, the temperature of the strip when entering the zinc pot is 571°C, and the temperature of the zinc pot is 585°C, the distance between the front air knife, the rear air knife and the strip is 2.0 cm, and the opening range of the cooling fan is 20%, and the air flow rate is 18000m 3 / h. The color-coated plate produced in this embodiment has good processing performance and meets the processing and molding requirements of various tile types; the corrosion resistance is 3-5 times that of ordinary products, and the service life is more than doubled when used in C3 and above corrosive environments.

[0033] In the cleaning process steps of this embodiment, the strip steel is subjected to two alkali washes, the alkali concentration is 0.5% to 1.5%, and the alkali temperature is 45°C to 60°C; the steel plate after alkali washing is then subjected to three water washes, the water washing temperature is 40°C to 65°C, wherein the last water wash uses desalted water, and the conductivity of the desalted water is ≤0.2ms / cm. Specifically, in this embodiment, the alkali concentration is 0.6%, the alkali temperature is 52°C, and the water washing temperature is 45°C.

[0034] In the passivation process, a layer of water-soluble organic polymer containing titanic acid and phosphate is coated on the surface of the steel strip, and after drying in a curing furnace at 80°C to 100°C, a passivation layer with a film thickness of 0.5 μm to 1.0 μm is formed. Specifically, in this embodiment, the temperature of the passivation curing furnace is 80°C, and the film thickness of the passivation layer is 0.5 μm.

[0035] After passivation, the strip enters the roller coating room for the initial primer coating. The primer coating viscosity is 8s to 20s (Zahn 4# viscosity cup). The primer coating is applied to the surface of the strip by continuous two-roll reverse coating. Then it enters the curing furnace for drying. The curing time in the curing furnace is controlled to be ≤35s, and the curing PMT temperature is ≤232°C. After the strip exits the curing furnace, it enters the water quenching tank and is then dried by cold air. The thickness of the primer film formed is 5μm to 15μm. Specifically, in this embodiment, the curing time in the primer curing furnace is 30s, the curing PMT temperature is 232°C, and the thickness of the primer film formed is 5μm.

[0036] When the steel strip after primer coating is applied with topcoat, the viscosity of the topcoat is 15s to 30s (Zahn 4# viscosity cup), and the topcoat is applied to the surface of the strip by continuous three-roll reverse coating, and then enters the curing furnace for drying, and the curing time is controlled to be ≤33s, and the curing PMT temperature is ≤241°C; after the strip exits the curing furnace, it enters the water quenching tank, and then is dried by cold air to form a topcoat dry film thickness of 15μm to 25μm. Specifically, in this embodiment, the curing time of the topcoat curing furnace is 30s, the curing PMT temperature is 232°C, and the topcoat dry film thickness is 19μm.

[0037] In this embodiment, the coating material is modified to improve the chemical corrosion resistance and processing performance:

[0038] (1) The topcoat uses a polyester resin with multiple terminal hydroxyl groups, and the ratio of the polyester resin with multiple terminal hydroxyl groups to the linear polyester resin in the topcoat is 1:4 to 1:2, and the content of the anti-corrosion additive in the topcoat is 15% to 20%. The linear polyester resin is grafted and strengthened at a ratio of 1:4 to 1:2, and the number of hydroxyl groups is increased by 10%, thereby increasing the cross-linking density of the film-forming material, thereby improving the solvent resistance of the system, and effectively improving the corrosion resistance of the paint film to corrosive media; at the same time, 15% to 20% of the anti-corrosion additive is added to the film-forming material to further strengthen the chemical resistance to oxidizing media and acidic and alkaline media. Specifically, the ratio of the polyester resin with multiple terminal hydroxyl groups to the linear polyester resin in the topcoat of this embodiment is 1:4, and at the same time, 15% of the anti-corrosion additive is added to the film-forming material.

[0039] (2) The pigments and fillers in the topcoat are treated with ultrafine dispersion to achieve a nanoscale pigment and filler ratio of ≥80% in the topcoat. The topcoat contains a fluoride as a high-temperature melting sealing material, which continuously seals the solvent voids formed by solvent volatilization during the high-temperature curing process of the coating. Improve the corrosion resistance and processability of the coating. Optimize the pigment-to-base ratio of the topcoat, and control the ratio of light-colored coating resin to pigments and fillers in the topcoat to ≤0.8, thereby improving the flexibility of the coating and meeting the requirements of complex molding and processing. Specifically, the nanoscale pigment and filler in the topcoat of this embodiment accounts for 80%, and the ratio of light-colored coating resin to pigments and fillers in the topcoat is 0.8.

[0040] (3) The primer adopts a polyurethane coating system with high corrosion resistance. By optimizing the cross-linking agent, the active substituent groups of the coating are fully cross-linked during the curing process, and the molecular space is tightly arranged, which effectively prevents the acid and alkali medium molecules from penetrating and diffusing into the interior of the paint film.

[0041] In this embodiment, the primer uses phosphate anti-rust color filler. Phosphate releases phosphate during the slow hydrolysis process. The phosphate ions combine with metal ions to form a dense and strong complex protective film with strong adhesion, which plays a role in protecting the metal surface, improving the corrosion resistance of the color-coated plate, and achieving chromium-free and environmentally friendly.

[0042] In this embodiment, in order to solve the difficult problems of cracking of complex cold-formed coatings and low acid and alkali corrosion resistance of coatings, the process design and optimization of steel plates and coating components are used to modify the coating pigments and fillers to increase the chemical inertness of the coating in acidic and alkaline environments. The cross-linking density and density of the coating are increased by optimizing the design of the coating system and the coating structure as well as optimizing the coating curing process, thereby improving the corrosion resistance and penetration of the coating to oxidative media, and manufacturing highly corrosion-resistant and environmentally friendly color-coated plates that meet the requirements of complex cold-formed processing. The plates can be used in building envelope systems in complex corrosive environments and can extend the service life of buildings by more than 20 years.

[0043] Table 1 shows the coating and coating compositions of Examples 1 to 3 and Comparative Examples 1 and 2

[0044] Serial number Mg content ratio of plating layer Corrosion resistant additive ratio Nano-filler ratio Color base ratio Primer coating pigment Example 1 1.2% 0.15 0.8 0.8 Phosphate Example 2 1.8% 0.18 0.85 0.70 Phosphate Example 3 1.5% 0.20 0.9 0.75 Phosphate Comparative Example 1 0 0.1 0.75 0.85 chromate Comparative Example 2 0 0 0.7 0.9 chromate

[0045] Table 2 shows the production process in Examples 1 to 3 and Comparative Examples 1 and 2.

[0046]

[0047] Table 3 shows the general properties of the color-coated plates in Examples 1-3 and Comparative Examples 1-2 (test method according to GB / T13448)

[0048] Serial number Total film thickness, μm T bend (crack) Shock Pencil hardness MEK Example 1 24 4T 9J F ≥100 Example 2 22 4T 9J F ≥100 Example 3 25 3T 9J F ≥100 Comparative Example 1 24 5T 6J H ≥100 Comparative Example 2 25 6T 6J H ≥100

[0049] Table 4 shows the unconventional properties of the color coated plates in Examples 1 to 3 and Comparative Examples 1 and 2.

[0050] Serial number 5% hydrochloric acid (V:V) 5% sodium hydroxide (m:m) Neutral salt spray (flat edge sealing) UV aging (UVB-313) Environmental performance Example 1 300h foaming ≤2S2 300h foaming ≤2S2 3000h≤2S2 800h color change ≤ 2 levels ROHS compliant Example 2 300h foaming ≤2S2 300h foaming ≤2S2 3000h≤2S2 800h color change ≤ 2 levels ROHS compliant Example 3 300h foaming ≤2S2 300h foaming ≤2S2 3000h≤2S2 800h color change ≤ 2 levels ROHS compliant Comparative Example 1 24h foaming ≤ 2S2 24h foaming ≤ 2S2 1500h≤2S2 600h color change ≤ 2 levels Not ROHS compliant Comparative Example 2 24h foaming ≤ 2S2 24h foaming ≤ 2S2 2000h≤2S2 600h color change ≤ 2 levels Not ROHS compliant

[0051] Through the analysis of the results of Examples 1-3 and Comparative Examples 1-2, compared with Comparative Examples 1 and 2, the processing flexibility of the color-coated steel plates of Examples 1-3 is improved by 1 to 3T; the acid and alkali resistance and other properties are improved by more than 10 times; and the environmental protection performance meets the ROHS requirements.

[0052] Example 2

[0053] A cold-formed high corrosion-resistant color-coated steel plate in this embodiment is basically consistent with Example 1, except that it includes the following chemical components in weight percentage: C: 0.10%, Si: 0.10%, Mn: 0.40%, P: 0.030%, S: 0.025%, and the rest is Fe and other inevitable impurities.

[0054] The double-sided coating weight of the high corrosion-resistant color-coated steel plate in this embodiment is ≥100g / m 2 , wherein the coating composition includes the following chemical components in weight percentage: Mg: 1.8%, Si: 2%, Al: 55%, and the rest is Zn.

[0055] A production method of a cold-formed high-corrosion-resistant color-coated steel plate of the present embodiment is produced by a two-coating and two-baking method, and includes the following process flow: hot-dip galvanized aluminum-magnesium substrate → cleaning → passivation → drying → initial coating of front primer / back primer → curing → water cooling → fine coating of front topcoat / back topcoat → curing → water cooling → inspection → coiling, wherein in the hot-dip galvanized aluminum-magnesium substrate process step, the temperature of the strip entering the zinc pot is controlled to be 575°C, and the temperature of the zinc pot is 585°C, the distance between the front air knife, the rear air knife and the strip is 2.2 cm, and the opening range of the cooling fan is 24%, and the air flow rate is 20000m 3 / h.

[0056] In the cleaning process steps of this embodiment, the strip steel is subjected to two alkali washes with an alkali solution concentration of 1.1% and an alkali solution temperature of 55°C; the steel plate after alkali washing is then subjected to three water washes with a water washing temperature of 55°C, wherein the last water wash uses desalted water with an electrical conductivity of ≤0.2ms / cm.

[0057] In the passivation process step, a layer of water-soluble organic polymer containing titanic acid and phosphate is coated on the surface of the strip, and after drying in a curing furnace at 85° C., a passivation layer with a film thickness of 1.0 μm is formed.

[0058] In this embodiment, the curing time in the primer curing furnace is 33s, the curing PMT temperature is 232°C, and the thickness of the primer film formed is 7μm. In this embodiment, the curing time in the topcoat curing furnace is 33s, the curing PMT temperature is 241°C, and the topcoat dry film thickness is 15μm.

[0059] The ratio of the polyester resin with multiple terminal hydroxyl groups to the linear polyester resin in the topcoat of this embodiment is 1:2, and 18% of the anti-corrosion additive is added to the film-forming material. The nano-scale pigments and fillers in the topcoat of this embodiment account for 85%, and the ratio of the light-colored coating resin to the pigments and fillers in the topcoat is 0.7.

[0060] Example 3

[0061] A cold-formed high corrosion-resistant color-coated steel plate in this embodiment is basically consistent with Example 1, except that it includes the following chemical components in weight percentage: C: 0.03%, Si: 0.09%, Mn: 0.46%, P: 0.032%, S: 0.029%, and the rest is Fe and other inevitable impurities.

[0062] The double-sided coating weight of the high corrosion-resistant color-coated steel plate in this embodiment is ≥100g / m 2 , wherein the coating composition includes the following chemical components in weight percentage: Mg: 1.5%, Si: 1.3%, Al: 53%, and the rest is Zn.

[0063] A production method of a cold-formed high-corrosion-resistant color-coated steel plate of the present embodiment is produced by a two-coating and two-baking method, and includes the following process flow: hot-dip galvanized aluminum-magnesium substrate → cleaning → passivation → drying → initial coating of front primer / back primer → curing → water cooling → fine coating of front topcoat / back topcoat → curing → water cooling → inspection → coiling, wherein in the hot-dip galvanized aluminum-magnesium substrate process step, the temperature of the strip entering the zinc pot is controlled to be 575°C, and the temperature of the zinc pot is 590°C, the distance between the front air knife, the rear air knife and the strip is 2.5 cm, and the opening range of the cooling fan is 30%, and the air flow rate is 22000m 3 / h.

[0064] In the cleaning process steps of this embodiment, the strip steel is subjected to two alkali washes with an alkali solution concentration of 1.5% and an alkali solution temperature of 60°C; the steel plate after alkali washing is then subjected to three water washes with a water washing temperature of 60°C, wherein the last water wash uses desalted water with an electrical conductivity of ≤0.2ms / cm.

[0065] In the passivation process, a layer of water-soluble organic polymer containing titanic acid and phosphate is coated on the surface of the strip, and after drying in a curing furnace at 95° C., a passivation layer with a film thickness of 0.8 μm is formed.

[0066] In this embodiment, the curing time in the primer curing furnace is 35s, the curing PMT temperature is 216°C, and the thickness of the primer film formed is 10μm. In this embodiment, the curing time in the topcoat curing furnace is 35s, the curing PMT temperature is 232°C, and the topcoat dry film thickness is 15μm.

[0067] The ratio of the polyester resin with multiple terminal hydroxyl groups to the linear polyester resin in the topcoat of this embodiment is 1:3, and 20% of the anti-corrosion additive is added to the film-forming material. The nanoscale pigments and fillers in the topcoat of this embodiment account for 90%, and the ratio of the light-colored coating resin to the pigments and fillers in the topcoat is 0.75.

[0068] Comparative Example 1

[0069] The color-coated steel plate of this comparative example includes the following chemical components in weight percentage: C: 0.15%, Si: 0.20%, Mn: 0.35%, P: 0.03%, S: 0.03%, and the rest is Fe and other inevitable impurities.

[0070] The coating composition of the color-coated steel plate of this comparative example does not include Mg. The topcoat of this comparative example adds 10% of anti-corrosion additives to the film-forming material. The nano-scale pigments and fillers in the topcoat of this embodiment account for 75%, and the ratio of light-colored coating resin to pigments and fillers in the topcoat is 0.85.

[0071] The production method of the color-coated steel plate in this comparative example adopts a two-coating and two-baking method, including the following process flow: hot-dip galvanized aluminum-magnesium substrate → cleaning → passivation → drying → initial coating of front primer / back primer → curing → water cooling → fine coating of front topcoat / back topcoat → curing → water cooling → inspection → coiling, wherein in the hot-dip galvanized aluminum-magnesium substrate process step, the temperature of the strip entering the zinc pot is controlled to be 575°C, and the temperature of the zinc pot is 595°C.

[0072] In the cleaning process of this comparative example, the strip steel was subjected to two alkali washes, the alkali concentration was 1.0%, and the alkali temperature was 60° C. The steel plate after alkali washing was then subjected to three water washes, and the water washing temperature was 60° C. In the passivation process, the temperature of the passivation curing furnace was 85° C., and the film thickness of the passivation layer was 0.5 μm.

[0073] In this comparative example, the curing time in the primer curing furnace is 35s, the curing PMT temperature is 232°C, and the thickness of the primer film formed is 10μm. In this comparative example, the curing time in the topcoat curing furnace is 35s, the curing PMT temperature is 241°C, and the topcoat dry film thickness is 15μm.

[0074] Comparative Example 2

[0075] The color-coated steel plate of this comparative example includes the following chemical components in weight percentage: C: 0.10%, Si: 0.25%, Mn: 0.30%, P: 0.03%, S: 0.03%, and the rest is Fe and other inevitable impurities.

[0076] The coating composition of the color-coated steel plate of this comparative example does not include Mg. The topcoat of this comparative example does not add anti-corrosion additives to the film-forming material. The nano-scale pigments and fillers in the topcoat of this embodiment account for 70%, and the ratio of light-colored coating resin to pigments and fillers in the topcoat is 0.9.

[0077] The production method of the color-coated steel plate in this comparative example adopts a two-coating and two-baking method, including the following process flow: hot-dip galvanized aluminum-magnesium substrate → cleaning → passivation → drying → initial coating of front primer / back primer → curing → water cooling → fine coating of front topcoat / back topcoat → curing → water cooling → inspection → coiling, wherein in the hot-dip galvanized aluminum-magnesium substrate process step, the temperature of the strip entering the zinc pot is controlled to be 580°C, and the temperature of the zinc pot is 600°C.

[0078] In the cleaning process of this comparative example, the strip steel was subjected to two alkali washes, the alkali concentration was 0.4%, and the alkali temperature was 50° C. The steel plate after alkali washing was then subjected to three water washes, and the water washing temperature was 50° C. In the passivation process, the temperature of the passivation curing furnace was 75° C., and the film thickness of the passivation layer was 0.8 μm.

[0079] In this comparative example, the curing time in the primer curing furnace is 40s, the curing PMT temperature is 241°C, and the thickness of the primer film formed is 15μm. In this comparative example, the curing time in the topcoat curing furnace is 40s, the curing PMT temperature is 249°C, and the topcoat dry film thickness is 18μm.

[0080] The examples described in the present invention are merely descriptions of the preferred implementation modes of the present invention, and are not intended to limit the concept and scope of the present invention. Without departing from the design concept of the present invention, various modifications and improvements made to the technical solutions of the present invention by engineers and technicians in this field should all fall within the protection scope of the present invention.

Claims

1. A cold-formed high corrosion-resistant color-coated steel sheet, characterized in that: The chemical composition includes the following weight percentages: C: 0.01% to 0.10%, Si: 0.08% to 0.10%, Mn: 0.40% to 0.50%, P: 0.030% to 0.035%, S: 0.025% to 0.035%, and the rest is Fe and other inevitable impurities; The double-sided coating weight of high corrosion resistant color-coated steel sheet is ≥100g / m 2 , the coating composition includes the following chemical components in weight percentage: Mg: 1% to 2%, Si: 1% to 2%, Al: 50% to 55%, and the rest is Zn; The production process of the color-coated steel plate includes the following process flow: hot-dip galvanizing aluminum-magnesium substrate→cleaning→passivation→drying→preliminary coating of front primer / back primer→curing→water cooling→fine coating of front topcoat / back topcoat→curing→water cooling→inspection→coiling, wherein in the hot-dip galvanizing aluminum-magnesium substrate process step, the temperature of the strip entering the zinc pot is controlled within the range of 575±5°C, and the temperature of the zinc pot is controlled within the range of 585±5°C; Among them, in the process steps of hot-dip galvanizing aluminum-magnesium substrate, the distance between the front air knife, the rear air knife and the strip steel is controlled to be 2.0cm~2.5cm, and the opening range of the cooling fan is 20%~30%, and the air flow rate is 18000m 3 / h~22000m 3 / h; the ratio of multi-terminal hydroxyl polyester resin to linear polyester resin in the topcoat is 1:4 to 1:2, and the content of anti-corrosion additives in the topcoat is 15% to 20%; the nano-scale pigments and fillers in the topcoat coating account for more than 80%; the topcoat contains a fluoride as a high-temperature melting sealing material, and the ratio of light-colored coating resin to pigments and fillers in the topcoat coating is controlled to be ≤0.

8.

2. A method for producing a cold-formed high corrosion-resistant color-coated steel sheet as claimed in claim 1, characterized in that: The process includes the following steps: hot-dip galvanized aluminum-magnesium substrate → cleaning → passivation → drying → initial coating of front primer / back primer → curing → water cooling → fine coating of front topcoat / back topcoat → curing → water cooling → inspection → coiling, wherein in the process steps of hot-dip galvanized aluminum-magnesium substrate, the temperature of the strip entering the zinc pot is controlled within the range of 575±5℃, and the temperature of the zinc pot is controlled within the range of 585±5℃.

3. The method for producing a cold-formed high corrosion-resistant color-coated steel sheet according to claim 2, characterized in that: In the cleaning process, the strip steel undergoes two alkali washes with an alkali solution concentration of 0.5% to 1.5% and an alkali solution temperature of 45°C to 60°C; the steel plate after alkali washing undergoes three water washes with a water washing temperature of 40°C to 65°C, wherein the last water wash uses desalted water with an electrical conductivity of ≤0.2ms / cm.

4. The method for producing a cold-formed high corrosion-resistant color-coated steel sheet according to claim 2, characterized in that: In the passivation process, a layer of water-soluble organic polymer containing titanic acid and phosphate is coated on the surface of the steel strip, and after being dried in a curing furnace at 80°C to 100°C, a passivation layer with a film thickness of 0.5μm to 1.0μm is formed.

5. The method for producing a cold-formed high corrosion-resistant color-coated steel sheet according to claim 2, characterized in that: The passivated strip enters the roller coating room for initial primer coating. The coating viscosity of the primer is 8s to 20s. The primer is applied to the surface of the strip by continuous two-roll reverse coating. The strip then enters the curing furnace for drying. The curing time in the curing furnace is controlled to be ≤35s, and the curing PMT temperature is ≤232°C. After exiting the curing furnace, the strip enters the water quenching tank and is then dried by cold air. The thickness of the primer film formed is 5μm to 15μm.

6. A method for producing a cold-formed high corrosion-resistant color-coated steel sheet according to any one of claims 2 to 5, characterized in that: When the steel strip is coated with topcoat after the primer is applied, the topcoat has a viscosity of 15s to 30s and is coated with three continuous rollers in reverse. Apply the topcoat coating on the surface of the strip, and then put it into the curing furnace for drying, controlling the curing time to ≤33s and the curing PMT temperature to ≤241℃; After the steel strip leaves the curing furnace, it enters the water quenching tank and is then dried by cold air to form a topcoat dry film with a thickness of 15μm to 25μm.

Citation Information

Patent Citations

  • Corrosion-resistant composite color-coated sheet and preparation method thereof

    CN112795279A

  • Environment-friendly PCM color precoated plate and preparation method thereof

    CN113954458A

  • High-corrosion-resistance deep-drawing color-coated sheet for outdoor household appliances and preparation method thereof

    CN114535036A

  • High-elongation hot-dipped aluminum-zinc and color coated steel plate with yield strength being 500 MPa and manufacturing method thereof

    CN105063484A

  • Hot-dipping Zn-Al-Mg alloy coating layer steel plate and preparation method thereof

    CN111270182A