AI Technical Summary
[0003]目前国内所使用的车轴用钢主要分为碳素结构钢和合金结构钢两类,碳素结构钢主要有35钢、40钢、45钢、50钢等,随着碳含量的升高,钢的强度增加,塑性降低,碳素结构钢的优势在于成本较低,价格低廉,成分体系简单,生产工艺控制较容易,但碳素结构钢整体上强度偏低,任性也较差,只可在低速低载重的车轴上使用
Smart Images

Figure CN116815048B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of special steel production, and in particular relates to alloy structural steel for railway axles and a preparation method thereof. Background Art
[0002] The axle of a railway train is an important part of its running part. Its quality determines the speed of the train and the safety of transportation. Therefore, the railway axle is a very important component. Since the axle is subjected to periodic alternating loads such as bending load, torsion load and composite load, the stress state is very complex and needs to withstand certain impact loads. The axle may break due to fatigue, bending, torsion or tensile stress during operation. For the selection of axle materials, the most important indicator is to ensure that it has good strength and certain toughness.
[0003] At present, the axle steels used in China are mainly divided into two categories: carbon structural steel and alloy structural steel. The main carbon structural steels include 35 steel, 40 steel, 45 steel, 50 steel, etc. As the carbon content increases, the strength of the steel increases and the plasticity decreases. The advantages of carbon structural steel are low cost, low price, simple composition system, and easier production process control. However, carbon structural steel has low strength overall and poor flexibility, and can only be used on low-speed and low-load axles.
[0004] The alloy structural steel axles mainly include 25CrMoA, 30CrMoA, 35CrMoA, 42CrMoA, and 30CrNi3MoV. Among them, chromium and molybdenum are added to 25-42CrMoA, which can improve the hardenability, strength and toughness of steel, improve thermal strength and fatigue performance, but chromium can significantly increase the tough-brittle transition temperature of steel and promote the temper brittleness of steel. Therefore, the low-temperature impact of steel is poor, and the axles produced cannot run stably at lower temperatures. 30CrNi3MoV reduces the amount of chromium added, adds nickel and vanadium elements, and improves the low-temperature impact performance of steel, but this type of steel adds precious alloys of nickel and vanadium, which increases the cost and makes the production process control more complicated. Summary of the invention
[0005] In order to overcome the defects of the above-mentioned prior art, the purpose of the present invention is to provide an alloy structural steel for railway axles and a preparation method. The alloy structural steel for railway axles has significantly improved strength and toughness compared with the currently used carbon structural steel axles; it can replace the most widely used alloy structural steel axle 25CrMoA, and has improved low-temperature impact performance compared with 25CrMoA; compared with 30CrNi3MoV, the low-temperature impact performance of steel is improved by adding cheap elements such as manganese and chromium to replace precious alloy nickel and vanadium.
[0006] In order to achieve the above-mentioned invention object, the present invention provides an alloy structural steel for railway axles and a preparation method thereof, wherein the alloy structural steel is composed of the following chemical elements in percentage by weight: C: 0.24% to 0.28%, Si: 0.17% to 0.30%, Mn: 0.80% to 1.10%, P≤0.015%, S≤0.007%, Cr: 0.60% to 0.90%, Mo: 0.20% to 0.23%, Alt: 0.020% to 0.030%, Ca: 0.0020% to 0.0030%, and the remainder is iron and unavoidable impurities.
[0007] The composition design reasons of the above-mentioned alloy structural steel for railway axles are as follows:
[0008] C: A portion of carbon enters the steel matrix to play a role in solid solution strengthening, and the other portion combines with carbide-forming elements in the alloy elements to form alloy carbides. Carbides, as hard and brittle phases, further play a strengthening role. Increasing the carbon content in steel can increase the strength and hardness of the steel, but too much carbon will reduce its plasticity and toughness. Therefore, the present invention chooses to add a carbon content of 0.24% to 0.28%.
[0009] Si: Silicon can improve the hardness of steel, but adding too much will reduce the plasticity and toughness of the steel. Silicon is also an element added to steel as a deoxidizer during steelmaking. Therefore, the present invention selects to add silicon content of 0.17% to 0.30%.
[0010] Mn: Manganese can improve the strength and wear resistance of steel, weaken and eliminate the "hot brittleness" phenomenon of sulfur, and improve the hardenability of steel. Manganese also has a deoxidation effect in the steelmaking process. Manganese is also a carbide-forming element. Dispersed carbides can refine grains and improve strength and toughness. Therefore, the present invention selects to add a manganese content of 0.80% to 1.10%.
[0011] P: Although phosphorus can increase the strength and hardness of steel, it significantly reduces the plasticity and toughness of steel, especially at low temperatures. It makes the steel significantly brittle and produces cold brittleness. Too much phosphorus can also lead to structural segregation. Therefore, the phosphorus content of the present invention is controlled to ≤0.015%.
[0012] S: On the one hand, sulfur in steel forms low-melting-point compounds with iron, causing "hot brittleness" during hot working; on the other hand, it also reduces the cleanliness of the steel, causing the risk of exceeding the inclusion standard. Therefore, the phosphorus content of the present invention is controlled at ≤0.007%.
[0013] Cr: Part of chromium in steel dissolves in iron to form a solid solution, and part of it forms carbides and alloy carbides with carbon and other alloy elements. Chromium is a medium carbide-forming element. Chromium carbides can be finely and evenly distributed in the volume of steel to improve the strength, hardness, yield point and high wear resistance of the steel. However, chromium can significantly increase the tough-to-brittle transition temperature of steel and promote temper brittleness of steel. Therefore, the present invention selects to add chromium content of 0.60% to 0.90%.
[0014] Mo: Molybdenum plays a major role in solid solution strengthening and precipitation strengthening in steel, which can significantly improve the hardenability and thermal strength of steel, inhibit the segregation of impurity elements such as P and S at grain boundaries, reduce temper brittleness, and refine the grains of steel. Therefore, the present invention selects the addition of molybdenum content of 0.20% to 0.23%.
[0015] Alt: Aluminum is a commonly used deoxidizer in steel. It combines with nitrogen to form aluminum nitride, which can refine the grains, inhibit the aging of low-carbon steel, improve the toughness of steel at low temperatures, and improve the oxidation resistance, wear resistance and fatigue strength of steel. Therefore, the present invention selects to add an aluminum content of 0.020% to 0.030%.
[0016] Ca: Calcium is added during the steelmaking process and can combine with aluminum oxide to form calcium aluminate, which can improve the castability of molten steel and reduce the risk of nozzle nodules on the one hand, and improve the state of inclusions on the other hand, and can improve the impact toughness of steel. Therefore, the present invention selects the addition of calcium content of 0.0020% to 0.0030%.
[0017] The method for preparing the alloy structural steel for railway axles comprises the following steps: electric furnace smelting→LF furnace refining→VD furnace refining→continuous casting→heating→rolling.
[0018] A preparation method of the above-mentioned alloy structural steel for railway axles, further, in the electric furnace smelting process, the electric furnace smelting adopts an eccentric bottom steel-tapping electric furnace, adopts oxygen oxidation, foam slag throughout the process, the final carbon of steel-tapping is controlled at 0.10%≤C≤0.25%, the final phosphorus is controlled at P≤0.013%, the electric furnace steel-tapping temperature is controlled at 1640℃~1680℃, aluminum-iron alloy (2.5~3.5kg / t) is added as a pre-deoxidizer during the steel-tapping process, and when 1 / 4 of the steel is tapped, ferrosilicon, ferromanganese, ferrochrome and ferromolybdenum alloy are added for pre-alloying.
[0019] In the above technical scheme, further, in the LF furnace refining process, the LF furnace adopts diffusion deoxidation to make white slag. After the liquid slag is formed, 1-3 kg / t of the first batch of ferrosilicon powder is added for diffusion deoxidation, the furnace door is closed for 10 minutes, and the second batch is added, with a total addition amount of 2-4 kg / t. After 5 minutes, the slag whiteness and temperature meet the requirements and a sample is taken. After the sample is reported back, an Al wire is fed to adjust the Al content in the steel to more than 0.020%, the white slag time is ≥25 minutes, and the composition is finally adjusted to achieve the chemical composition of the present invention. Argon is blown at the bottom of the ladle for stirring to facilitate uniform composition and removal of non-metallic inclusions. The argon pressure is controlled at 0.2 MPa-0.4 MPa, and the LF furnace hanging ladle temperature is controlled at 1665°C-1695°C.
[0020] In the above technical scheme, further, in the VD furnace refining process, the temperature is controlled at 1630℃~1670℃ when entering VD, calcium treatment is carried out before the VD furnace is evacuated, and vacuum treatment is carried out after 2.0~2.4m / t of silicon calcium wire is fed, the vacuum degree is ≤100Pa, and the vacuum is maintained for 15min~25min. After breaking the vacuum, argon is blown statically for 15min~35min, and the argon pressure is maintained at 0.1Mpa~0.3Mpa. The slag surface moves slightly and the molten steel is not exposed. The temperature of the VD furnace hanging bag is controlled at 1557℃~1567℃.
[0021] In the above technical solution, further, in the continuous casting process, the superheat is ≤30°C to ensure casting at a lower superheat, and the crystallizer water flow rate is 170m 3 / h, crystallizer electromagnetic stirring current 375±20A, crystallizer uses low-carbon protective slag, secondary cooling water specific water volume 0.30±0.02L / kg, terminal electromagnetic stirring current 250±30A, casting speed 0.85~0.90m / min. In order to prevent oxidation during solidification of molten steel, long nozzle, submerged nozzle, tundish covering agent and other measures are adopted throughout the continuous casting process to protect the casting throughout the process, and low-carbon steel protective slag is used for the crystallizer protective slag.
[0022] In the above technical scheme, further, in the heating process, a heating furnace is used for heating, and a cold charging process is adopted, that is, the ingot is put into the furnace for heating only after it has cooled to room temperature. The temperature of the preheating section is less than 750°C, the temperature of the second section is 840°C~880°C, the temperature of the first section is 1190°C~1220°C, the temperature of the equalizing section is 1180°C~1210°C, and the total heating time is ≥210min to ensure that the temperature of the ingot is uniform and thoroughly burned.
[0023] In the above technical scheme, further, in the rolling process, the rolling adopts the primary rolling mill and the continuous rolling mill group, the starting rolling temperature is 1100℃~1200℃, the final rolling temperature is 800℃~850℃, the low final rolling temperature can inhibit the dynamic recrystallization of the steel and prevent the grain growth, the rolling specification range is φ45mm~φ85mm, to ensure that there is enough compression ratio from the steel billet to the rolled product, to prevent the steel from cracking due to the excessive cooling rate after rolling, the steel is cooled by stack cooling after rolling, the stacking temperature is ≥300℃, and the stacking time is ≥8h.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] ① The present invention ensures that the steel has good strength and plasticity through reasonable component design. The smelting adopts electric furnace smelting, LF and VD refining processes, and solidification adopts continuous casting. By setting the optimal process parameters, each process is optimally matched to improve the inclusion content and low-multiple quality of the steel. Through the continuous rolling process, the uniformity and low-multiple quality of the steel are further improved, the grain size grade is increased, and the performance of the steel is further improved.
[0026] ② The alloy structural steel for railway axles prepared by the present invention has significantly improved strength and toughness compared to the currently used carbon structural steel axles, while the cost is slightly increased. The alloy structural steel for railway axles of the present invention can mainly replace the most widely used alloy structural steel axle 25CrMoA, and has improved low-temperature impact performance compared to 25CrMoA without reducing other performance indicators.
[0027] ③ The alloy structural steel for railway axles of the present invention has a specification range of φ45mm~φ85mm, low-power indicators of general porosity ≤2.0 level, central porosity ≤2.0 level, ingot-shaped segregation ≤2.0 level, and spotted segregation ≤2.0 level; non-metallic inclusion indicators A fine ≤1.5 level, A coarse ≤2.0 level, B fine ≤1.5 level, B coarse ≤2.0 level, C fine ≤1.0 level, C coarse ≤1.0 level, D fine ≤1.5 level, D coarse ≤2.0 level, DS ≤2.0 level; yield strength ≥420MPa, tensile strength 650~800MPa, elongation ≥18%, cross-sectional shrinkage ≥60%, and impact energy at -20℃ ≥40J, which fully meets the use requirements of axle steel. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a low-magnification picture of Example 3;
[0029] Figure 2 Image of non-metallic inclusions in Example 3. DETAILED DESCRIPTION
[0030] The present invention is further described below in conjunction with specific examples, but the present invention is not limited in any way. To avoid redundant description, the raw materials in the following examples are all commercially available products unless otherwise specified, and the methods used are all conventional methods unless otherwise specified. Performance tests were performed according to standards GB / T 226, GB / T 228.1, GB / T 229, GB / T 1979, and GB / T 10561.
[0031] Example
[0032] The chemical composition of the embodiment of the present invention is shown in Table 1; the chemical composition satisfies C: 0.24-0.28%, Si: 0.17-0.30%, Mn: 0.80-1.10%, P≤0.015%, S≤0.007%, Cr: 0.60-0.90%, Mo: 0.20-0.23%, Alt: 0.020-0.030%, Ca: 0.0020-0.0030%. The electric furnace smelting process of the corresponding embodiment is shown in Table 2; the LF furnace refining process of the corresponding embodiment is shown in Table 3; the VD furnace refining process of the corresponding embodiment is shown in Table 4; the continuous casting process of the corresponding embodiment is shown in Table 5; the heating process of the corresponding embodiment is shown in Table 6; the rolling process of the corresponding embodiment is shown in Table 7; the low-power index of the corresponding embodiment is shown in Table 8; the non-metallic inclusion index of the corresponding embodiment is shown in Table 9; the mechanical properties of the corresponding embodiment and the comparative steel grade 25CrMoA are shown in Table 10. The low-power and non-metallic inclusions of Example 3 are as follows Figure 1 and Figure 2 shown.
[0033] Table 1 Chemical composition of the present invention by weight%
[0034]
[0035]
[0036] Table 2 Electric furnace smelting process of the embodiment of the present invention
[0037]
[0038] Table 3 LF furnace refining process of the embodiment of the present invention
[0039]
[0040] Table 4 VD furnace refining process of the embodiment of the present invention
[0041]
[0042] Table 5 Continuous casting process of the embodiment of the present invention
[0043]
[0044] Table 6 Heating process of the embodiment of the present invention
[0045]
[0046] Table 7 Rolling process of the embodiment of the present invention
[0047]
[0048] Table 8 Low magnification index of the embodiment of the present invention
[0049] Example General loose / grade Center looseness / level Ingot segregation / grade Spotty segregation / grade 1 0 0 0 0 2 0 0 0 0 3 0 0 0 0 4 0 0 0 0 5 0 0 0 0 6 0 0.5 0 0
[0050] Table 9 Non-metallic inclusion indicators of the embodiments of the present invention
[0051] Example A fine / grade A coarse / grade B fine / grade B coarse / grade C Fine / Grade C coarse / grade D Fine / Grade D Coarse / Grade DS / level 1 0.5 0 0 0.5 0 0 0 0 0 2 1.0 0 0.5 0 0 0 0 0 0 3 0.5 0.5 0 0 0 0 0.5 0 0 4 0.5 0 0 0 0 0 0 0 0 5 0.5 0 0.5 0 0 0 0 0 0.5 6 1.0 0 0 0 0 0 0 0 0
[0052] Table 10 Mechanical properties of the embodiments of the present invention and the comparative examples
[0053] Example Yield strength / MPa Tensile strength / MPa Elongation / % Sectional shrinkage / % Impact energy at -20℃ / J 1 480 730 25 66 56 2 465 742 26 67 55 3 468 735 23 65 53 4 470 741 25 67 58 5 475 745 27 68 54 6 468 738 26 66 55 Comparative Example Yield strength / MPa Tensile strength / MPa Elongation / % Sectional shrinkage / % Impact energy at -20℃ / J 25CrMoA 430 690 20 62 10
[0054] For any technician familiar with the art, without departing from the scope of the technical solution of the present invention, the technical content disclosed above can be used to make many possible changes and modifications to the technical solution of the present invention, or modified into equivalent embodiments with equivalent changes. Therefore, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention should still fall within the scope of protection of the technical solution of the present invention.
Claims
1. An alloy structural steel for railway axles, characterized in that: The alloy structural steel is composed of the following chemical elements in percentage by weight: C: 0.24% to 0.27%, Si: 0.17% to 0.26%, Mn: 1.01% to 1.10%, P≤0.013%, S≤0.005%, Cr: 0.70% to 0.90%, Mo: 0.21% to 0.23%, Alt: 0.021% to 0.030%, Ca: 0.0023% to 0.0030%, and the balance is iron and unavoidable impurities; The alloy structural steel for railway axles has a specification range of φ45mm to φ85mm, a low-power index of general porosity ≤2.0, a central porosity ≤2.0, an ingot-shaped segregation ≤2.0, and a spotted segregation ≤2.0; non-metallic inclusion index A fine ≤1.5, A coarse ≤2.0, B fine ≤1.5, B coarse ≤2.0, C fine ≤1.0, C coarse ≤1.0, D fine ≤1.5, D coarse ≤2.0, and DS ≤2.0; yield strength ≥465MPa, tensile strength 730-800MPa, elongation ≥23%, cross-sectional shrinkage ≥65%, and impact energy at -20°C ≥53J; A method for preparing the above alloy structural steel for railway axles, the method comprising the following steps: electric furnace smelting → LF furnace refining → VD furnace refining → continuous casting → heating → rolling; Among them, in the VD furnace refining process, the VD inlet temperature is controlled at 1630℃~1670℃, 2.0~2.4m / t of calcium silicon wire is fed into the VD furnace before vacuuming, and then vacuum treatment is carried out, the vacuum degree is ≤100Pa, and argon is blown for 15~35min after breaking the vacuum, the argon pressure is 0.1~0.3Mpa, and the VD furnace hanging bag temperature is controlled at 1557℃~1567℃; In the continuous casting process, the superheat is ≤30℃, the electromagnetic stirring current of the crystallizer is 375±20A, the crystallizer uses low-carbon protective slag, the secondary cooling water volume is 0.30±0.02L / kg, the terminal electromagnetic stirring current is 250±30A, and the casting speed is 0.85~0.90m / min.
2. The alloy structural steel for railway axles according to claim 1, characterized in that: In the electric furnace smelting process, an eccentric bottom steel-tapping electric furnace is used, oxygen oxidation is adopted, foamy slag is used throughout the process, the final carbon of steel-tapping is controlled at 0.10%≤C≤0.25%, the final phosphorus is controlled at P≤0.013%, the electric furnace steel-tapping temperature is controlled at 1640℃~1680℃, and aluminum-iron alloy is added during the steel-tapping process.
3. The alloy structural steel for railway axles according to claim 2, characterized in that: In the LF furnace refining process, diffusion deoxidation is used to make white slag. After the liquid slag is formed, the first batch of diffusion deoxidizer ferrosilicon powder is added, the furnace door is closed for 10 minutes, and the second batch is added. The total amount added is 2-4kg / t; the white slag time is ≥25min, argon is blown from the bottom of the ladle for stirring, the argon pressure is controlled at 0.2-0.4MPa, and the LF furnace hanging ladle temperature is controlled at 1665℃~1695℃.
4. The alloy structural steel for railway axles according to claim 3, characterized in that: In the heating process, heating furnace heating and cold charging process are adopted, the preheating section temperature is less than 750℃, the second section temperature is 840℃~880℃, the first section temperature is 1190℃~1220℃, the soaking section temperature is 1180℃~1210℃, and the total heating time is ≥210min.
5. The alloy structural steel for railway axles according to claim 4, characterized in that: In the rolling process, a primary rolling mill and a continuous rolling mill are used, the starting rolling temperature is 1100℃~1200℃, the final rolling temperature is 800℃~850℃, and the steel is cooled by stack cooling after rolling, the stacking temperature is ≥300℃, and the stacking time is ≥8h.