A preparation method, product and application of ternary nanowire positive electrode material

The ternary nanowire positive electrode material was prepared by surfactant-free and mild chemical solution methods, which solved the problem of poor electrochemical performance of the ternary material and achieved the performance of lithium-ion battery with high specific energy and good cycle stability.

CN116835671BActive Publication Date: 2024-11-08SHANGHAI NAT ENG RES CENT FORNANOTECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310917110.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-25
Publication Date
2024-11-08
Estimated Expiration
2043-07-25

AI Technical Summary

Technical Problem

The electrochemical performance of existing ternary materials is insufficient and it is difficult to meet the needs of high-specific energy lithium-ion batteries.

Method used

The ternary nanowire positive electrode material is prepared by surfactant-free and gentle chemical solution methods. Through specific solution composition and heat treatment steps, a nanowire structure with a large specific surface area is formed, which improves the contact between the material and the electrolyte and improves electrochemistry. performance.

Benefits of technology

The high initial discharge specific capacity and good cycle stability under 1C ratio conditions were achieved. The first discharge specific capacity was 178.9 mAh/g, and the capacity retention rate was 95.1% after 50 cycles, which significantly improved the electrochemical performance of the battery. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116835671B_ABST
    Figure CN116835671B_ABST
Patent Text Reader

Abstract

The present invention provides a preparation method of a ternary nanowire positive electrode material, a product and an application thereof. The present invention uses a surfactant-free and mild chemical solution method to prepare the ternary nanowire. The structure has a large specific surface area and can fully contact with the electrolyte, thereby improving the electrochemical performance of the material. Under the 1C rate charge and discharge condition, the first discharge specific capacity is 178.9 mAh / g. After 50 cycles, the discharge specific capacity is 170.2 mAh / g, and the capacity retention rate is 95.1%. In addition, the preparation method is simple, the process conditions are easy to achieve, the energy consumption is low, and the preparation is pollution-free.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a preparation method of a lithium battery cathode material, in particular to a preparation method, product and application of a ternary nanowire cathode material. Background Art

[0002] With the rapid development of smaller, lighter and higher-performance electronic and communication devices, there are increasingly high requirements for the battery performance, especially the specific energy, for powering these devices. However, it is difficult to further improve the specific capacity of the commercially available lithium-ion batteries and MH / Ni batteries at present. Therefore, there is an urgent need to develop batteries with higher specific energy. As a high specific energy chemical power source, lithium-ion secondary batteries have been widely used in the fields of mobile communication, laptop computers, video cameras, cameras, portable instruments and meters, etc., and have rapidly developed into one of the most important secondary batteries at present. Lithium-ion batteries, as the latest generation of green high-energy storage batteries, have developed rapidly in the early 1990s. Lithium-ion batteries are favored because of their advantages such as high voltage, high energy density, long cycle life and low environmental pollution.

[0003] Ternary materials are called the preferred materials for lithium batteries because of their low price and stable performance. Since the ternary material LiNi 1-x-y Co x Mn y O2 (0 < x < 1, 0 < y < 1) has characteristics superior to those of lithium iron phosphate and lithium cobaltate, and different performance ternary electrode materials can be prepared by adjusting the ratios of nickel, cobalt and manganese. With the rise and development of new energy vehicles, ternary materials are a research hotspot.

[0004] The present invention provides a preparation method of a ternary nanowire cathode material (LiNi 1-x-y Co x Mn y O2 (0 < x < 1, 0 < y < 1)). The present invention uses a surfactant-free and a mild chemical solution method to prepare ternary nanowires. This structure has a large specific surface area, can fully contact with the electrolyte, and thus can improve the electrochemical performance of the material. And the preparation method is simple, the process conditions are easy to realize, the energy consumption is low, and the preparation is pollution-free. Summary of the Invention

[0005] To overcome the deficiency of poor electrochemical performance of ternary materials, the purpose of the present invention is to provide a preparation method of a ternary nanowire cathode material.

[0006] Another purpose of the present invention is to provide a ternary nanowire cathode material product obtained by the above method.

[0007] Still another purpose of the present invention is to provide an application of the above product.

[0008] The object of the present invention is achieved through the following solution: A preparation method of a ternary nanowire cathode material, which uses a surfactant-free and a mild chemical solution method to prepare ternary nanowires. The specific steps of this method are as follows:

[0009] (1) Add 5 mL of acetylacetone and 10 mL of hydrazine hydrate sequentially to a 200 mL conical flask containing a solution of lithium salt, nickel salt, cobalt salt, and manganese salt, with a molar ratio of 1: 1 - x - y: x: y, and stir magnetically at 90 - 110 °C for 0.5 - 1 h;

[0010] (2) Reflux the solution at 90 - 110 °C for 24 - 36 h, then filter the precursor, wash it 3 - 5 times with water and absolute ethanol; then dry it at 60 - 80 °C;

[0011] (3) Place the precursor in a muffle furnace and calcine it at 550 - 650 °C for 1 - 2 h at a heating rate of 1 - 2 °C / min to obtain the final product.

[0012] The lithium salt is one or a combination of lithium acetate, lithium nitrate, or lithium chloride.

[0013] The nickel salt is one or a combination of nickel acetate, nickel nitrate, or nickel chloride.

[0014] The cobalt salt is one or a combination of cobalt acetate, cobalt nitrate, or cobalt chloride.

[0015] The manganese salt is one or a combination of manganese acetate, manganese nitrate, or manganese chloride.

[0016] The present invention provides a ternary nanowire cathode material prepared according to any one of the above methods.

[0017] The present invention provides an application of a ternary nanowire cathode material in a lithium-ion battery.

[0018] The present invention provides a preparation method of a ternary nanowire cathode material (LiNi 1-x-y Co x Mn y O2 (0 < x < 1, 0 < y < 1)). The present invention uses a surfactant-free and a mild chemical solution method to prepare ternary nanowires. This structure has a large specific surface area, can fully contact with the electrolyte, and thus can improve the electrochemical performance of the material. And the preparation method is simple, the process conditions are easy to achieve, the energy consumption is low, and the preparation is pollution-free. Under the condition of 1C charge-discharge rate, the initial discharge specific capacity is 178.9 mAh / g. After 50 cycles, the discharge specific capacity is 170.2 mAh / g, and the capacity retention rate is 95.1%. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 For example 1 ternary nanowire LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 XRD pattern of O2 material;

[0020] Figure 2 For example 2 ternary nanowire LiNi 0.5 Co 0.3 Mn 0.2 SEM image of O2 material;

[0021] Figure 3 For example 3 ternary nanowire LiNi 0.8 Co 0.1 Mn 0.1 Cycle life diagram of O2 material. DETAILED DESCRIPTION

[0022] The present invention is described in detail through the following specific examples, but the protection scope of the present invention is not limited to these embodiments.

[0023] Embodiment 1:

[0024] A ternary nanowire positive electrode material is prepared by using a surfactant-free and mild chemical solution method to prepare the ternary nanowires according to the following steps:

[0025] (1) Add 5 mL of acetylacetone and 10 mL of hydrazine hydrate to a conical flask containing 200 mL of a solution of lithium acetate, nickel acetate, cobalt acetate and manganese acetate in order to make the molar ratio 1: 0.333: 0.333:0.333, and stir magnetically at 90 °C for 1 h to obtain a solution;

[0026] (2) After the solution is refluxed at 90 °C for 36 h, the obtained product is filtered, washed with water and anhydrous ethanol for 3 to 5 times, and dried at 60 °C to obtain a precursor;

[0027] (3) The precursor was placed in a muffle furnace and calcined at 550 °C for 2 h at a heating rate of 1 °C / min to obtain the final product, a ternary nanowire positive electrode material.

[0028] Figure 1 It is a ternary nanowire LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 The XRD pattern of O2 material is compared with the literature, and the material is pure phase, and R (003) / (104) =1.7, greater than 1.2, indicating no Li + with Ni 2+The ion mixing phenomenon and the splitting peaks of (006) / (102) and (108) / (110) indicate that the material has a layered structure.

[0029] Embodiment 2:

[0030] A ternary nanowire positive electrode material is prepared in the following steps similar to those in Example 1:

[0031] (1) Add 5 mL of acetylacetone and 10 mL of hydrazine hydrate to a conical flask containing 200 mL of a solution of lithium nitrate, nickel nitrate, cobalt nitrate and nickel nitrate in order, wherein the molar ratio is 1: 0.5: 0.3: 0.2, and stir magnetically at 100 °C for 0.5 h to obtain a solution;

[0032] (2) Reflux the solution at 100 °C for 30 h, then filter the precursor, wash it with water and anhydrous ethanol five times, and then dry it at 80 °C;

[0033] (3) The precursor was placed in a muffle furnace and calcined at 650 °C for 1 h at a heating rate of 1 °C / min to obtain the final product LiNi 0.5 Co 0.3 Mn 0.2 O2 ternary nanowire materials.

[0034] Figure 2 Ternary nanowire LiNi 0.5 Co 0.3 Mn 0.2 SEM image of O2 material.

[0035] Embodiment three:

[0036] A ternary nanowire positive electrode material is prepared in the following steps similar to those in Example 1:

[0037] (1) Add 5 mL of acetylacetone and 10 mL of hydrazine hydrate to a conical flask containing 200 mL of a solution of lithium chloride, nickel chloride, cobalt chloride and nickel chloride in order, wherein the molar ratio is 1: 0.8: 0.1: 0.1, and stir magnetically at 100 °C for 0.5 h to obtain a solution;

[0038] (2) Reflux the solution at 110 °C for 24 h, then filter the precursor, wash it with water and anhydrous ethanol five times, and then dry it at 80 °C;

[0039] (3) The precursor was placed in a muffle furnace and calcined at 650 °C for 1 h at a heating rate of 1 °C / min to obtain the final product LiNi 0.8 Co 0.1 Mn 0.1O2 ternary nanowire materials.

[0040] Figure 3 Ternary nanowire LiNi 0.8 Co 0.1 Mn 0.1 The cycle life diagram of O2 material shows that under the 1C rate charge and discharge condition, the first discharge capacity is 178.9 mAh / g. After 50 cycles, the discharge capacity is 170.2 mAh / g, and the capacity retention rate is 95.1%.

Claims

1. A method for preparing a ternary nanowire positive electrode material, characterized in that The ternary nanowires were prepared using a surfactant-free and mild chemical solution method, comprising the following steps: (1) Add 5 mL of acetylacetone and 10 mL of hydrazine hydrate to a conical flask containing 200 mL of a solution of a lithium salt, a nickel salt, a cobalt salt and a manganese salt in order to make the molar ratio 1: 1-xy: x:y, and stir magnetically at 90-110 °C for 0.5-1 h to obtain a solution; (2) After the solution is refluxed at 90-110 °C for 24-36 h, the obtained product is filtered, washed with water and anhydrous ethanol for 3-5 times, and dried at 60-80 °C to obtain a precursor; (3) The precursor was placed in a muffle furnace and calcined at 550-650 °C for 1-2 h at a heating rate of 1-2 °C / min to obtain the ternary nanowire positive electrode material LiNi 1-x-y Co x Mn y O2,0 <x<1, 0<y<1; The lithium salt is one of lithium acetate, lithium nitrate or lithium chloride; The nickel salt is one of nickel acetate, nickel nitrate or nickel chloride; The cobalt salt is one of cobalt acetate, cobalt nitrate or cobalt chloride; The manganese salt is one of manganese acetate, manganese nitrate or manganese chloride.

2. The method for preparing a ternary nanowire positive electrode material according to claim 1, characterized in that: Prepare as follows: (1) Add 5 mL of acetylacetone and 10 mL of hydrazine hydrate to a conical flask containing 200 mL of a solution of lithium acetate, nickel acetate, cobalt acetate and manganese acetate in order to make the molar ratio 1: 0.333: 0.333:0.333, and stir magnetically at 90 °C for 1 h to obtain a solution; (2) After the solution is refluxed at 90 °C for 36 h, the obtained product is filtered, washed with water and anhydrous ethanol for 3 to 5 times, and dried at 60 °C to obtain a precursor; (3) The precursor was placed in a muffle furnace and calcined at 550 °C for 2 h at a heating rate of 1 °C / min to obtain the final product LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 ternary nanowire positive electrode material.

3. The method for preparing a ternary nanowire positive electrode material according to claim 1, characterized in that: Prepare as follows: (1) Add 5 mL of acetylacetone and 10 mL of hydrazine hydrate to a conical flask containing 200 mL of a solution of lithium nitrate, nickel nitrate, cobalt nitrate and nickel nitrate in order, wherein the molar ratio is 1: 0.5: 0.3: 0.2, and stir magnetically at 100 °C for 0.5 h to obtain a solution; (2) Reflux the solution at 100 °C for 30 h, then filter the precursor and wash it with water and anhydrous ethanol five times; Then dried at 80 °C; (3) The precursor was placed in a muffle furnace and calcined at 650 °C for 1 h at a heating rate of 1 °C / min to obtain the final product LiNi 0.5 Co 0.3 Mn 0.2 O2 ternary nanowire materials.

4. The method for preparing a ternary nanowire positive electrode material according to claim 1, characterized in that: Prepare as follows: (1) Add 5 mL of acetylacetone and 10 mL of hydrazine hydrate to a conical flask containing 200 mL of a solution of lithium chloride, nickel chloride, cobalt chloride and nickel chloride in order, wherein the molar ratio is 1: 0.8: 0.1: 0.1, and stir magnetically at 100 °C for 0.5 h to obtain a solution; (2) Reflux the solution at 110 °C for 24 h, then filter the precursor and wash it with water and anhydrous ethanol five times; Then dried at 80 °C; (3) The precursor was placed in a muffle furnace and calcined at 650 °C for 1 h at a heating rate of 1 °C / min to obtain the final product LiNi 0.8 Co 0.1 Mn 0.1 O2 ternary nanowire materials.

Citation Information

Patent Citations

  • Silver loaded mesoporous silicon oxide coated ternary cathode material, and preparation method and applications thereof

    CN106571455A

  • Nickel-cobalt-manganese ternary positive material for lithium-ion batteries, and preparation method of nickel-cobalt-manganese ternary positive material

    CN107445214A

  • Lithium ion battery ternary nanometer single crystal positive electrode material preparation method

    CN108123131A

  • Preparation method of enabling foamed nickel to grow ternary positive electrode material in-situ, product and application

    CN110931769A

  • Preparation method, product and application of ternary nano positive electrode material

    CN115947388A