Carbonized lightweight aggregate concrete and preparation method thereof
Carbonated lightweight aggregate concrete was prepared by combining low-calcium cement and modified bio-based aggregate with a carbonization curing process. This solved the problems of high energy consumption and high CO2 emissions in lightweight aggregate concrete, improved the mechanical properties and durability of concrete, and promoted sustainable development.
Patent Information
- Application Number
- CN202310566928.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-19
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-05-19
AI Technical Summary
The conventional silicate cement used in existing lightweight aggregate concrete has high energy consumption and high CO2 emissions, and the chemical process of the modified liquid is not easy to control, which affects the durability and mechanical properties of the concrete.
By using low-calcium cement and modified bio-based aggregates, combined with carbonation curing process, and taking advantage of the carbonation activity of low-calcium cement, the bonding between aggregates and cement paste is enhanced through the carbonation activity of cement-based materials on the surface of modified bio-based aggregates, thus preparing carbonized lightweight aggregate concrete.
It achieves low carbon emissions and resource conservation, improves the mechanical properties and durability of lightweight aggregate concrete, and promotes the sustainable development of concrete.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building materials, and particularly relates to a carbonized lightweight aggregate concrete and a preparation method thereof. Background Art
[0002] Lightweight aggregate concrete has the characteristics of low bulk density and excellent thermal insulation performance, which is significantly different from ordinary concrete. It has broad application prospects, especially in construction projects with special requirements for earthquake resistance, sound insulation and heat insulation.
[0003] General Portland cement used in lightweight aggregate concrete is a high-energy consumption, high-CO2 emission material that will cause great harm to the global environment. In addition, both natural lightweight aggregate and artificial lightweight aggregate require resource consumption in production and will also have an adverse impact on the environment. Therefore, expanding the application of low-calcium cement has received more and more attention, and finding alternative recycled aggregates has become a research hotspot.
[0004] Patent CN115340340A discloses a bio-based lightweight aggregate concrete and a preparation method thereof. The method modifies the bio-based aggregate by synthesizing a modifying liquid. The magnesium sulfate-magnesium oxide system in the modifying liquid is greatly affected by the environmental pH value, and the chemical process is difficult to control. The calcium sulfoxide generated with cement will affect the volume change of the concrete, thereby causing the durability and mechanical properties of the lightweight aggregate concrete to decrease. Summary of the invention
[0005] The purpose of the present invention is to provide a carbonized lightweight aggregate concrete and a preparation method thereof, which combines the water reservoir function of lightweight aggregate and synergistically utilizes the carbonation activity characteristics of low-calcium cement to ensure the continuity of low-calcium cement hydration and carbonation reaction; another purpose of the present invention is to use a modified bio-based aggregate surface cement-based material with a certain carbonation activity to further strengthen the connection between aggregate and cement stone, and the obtained lightweight aggregate concrete has good mechanical properties.
[0006] In order to achieve the above purpose, the technical solutions adopted are as follows:
[0007] A carbonized lightweight aggregate concrete is composed of the following raw materials in parts by weight: 270-500 parts of low-calcium cement, 500-650 parts of coarse aggregate, 410-600 parts of fine aggregate, 140-180 parts of water, 5-10 parts of carbonization enhancer, and 5-10 parts of water reducer;
[0008] The coarse aggregate is one of modified bio-based aggregate, fly ash ceramsite, shale ceramsite, and expanded perlite, and has a particle size of 5-20 mm;
[0009] The fine aggregate is one of natural river sand, machine-made sand, and modified bio-based aggregate, with a fineness modulus of 2.3 to 3.2 and a crushing value of ≤25%.
[0010] According to the above scheme, the modified bio-based aggregate is prepared in the following manner:
[0011] The biomass raw materials are soaked in a sodium hydroxide solution to remove surface oily impurities;
[0012] After taking out, crush, sieve and dry, heat treat at 60℃~80℃ for 30min~40min;
[0013] The interface modification slurry is added for roll coating, and CO2 is continuously introduced during the rolling coating process.
[0014] According to the above scheme, the biomass raw material includes any one of oil palm shell, peach shell, palm tree shell and coconut shell or a mixture thereof.
[0015] According to the above scheme, the interface modification slurry is mixed with concrete waste, water and dispersant; the mass ratio of water to concrete waste dry basis is (1-2): 1; the dispersant is polycarboxylate, and the dosage is 0.2%-0.4% of the total mass of the interface modification slurry;
[0016] The concrete waste is wastewater generated by cleaning concrete mixers, filter presses or concrete tankers, or waste slurry sediment generated by decomposition of waste concrete, and its dry basis components contain CaO 40-50wt%, SiO2 30~40wt%, and the rest are unavoidable impurities.
[0017] According to the above scheme, the low-calcium cement has C3S2, CS and C2S as the main mineral phases, with C3S2 15-60% by mass, CS 10-55% by mass, C2S 20-60% by mass, and the sum of the mass proportions of the three mineral phases ≥87%, a calcium-silicon ratio of 1.4-1.7, a 45μm negative pressure sieve residue ≤26%, and a specific surface area ≥350m 2 / kg.
[0018] According to the above scheme, the water reducer is a naphthalene-based water reducer, and its water reduction rate is 15-25%.
[0019] According to the above scheme, the carbonization enhancer is one of polyglucosamine and polyethylene glycol; the molecular weight of the polyglucosamine is 150,000 to 400,000, and the molecular weight of the polyethylene glycol is 300 to 600.
[0020] The method for preparing the carbonized lightweight aggregate concrete comprises the following steps:
[0021] 1) Soak the coarse aggregate in water for 2 hours and then drain it, keeping the surface of the coarse aggregate saturated and dry;
[0022] 2) Mix with fine aggregate in proportion for 30 seconds and premix evenly; then add low-calcium cement and stir for 60 seconds until the mixture is evenly mixed; finally add water and admixtures and stir for 60-120 seconds to obtain a lightweight concrete mixture;
[0023] 3) Pour into a mold for casting and forming, place in a CO2 curing environment for carbonization curing, and obtain a carbonized lightweight aggregate concrete product.
[0024] According to the above scheme, the carbonization curing system is: CO2 concentration 18~100vol%, curing temperature 30~70℃, curing pressure 0.1~1.0MPa, and curing time 6~24h.
[0025] According to the above scheme, the CO2 curing environment adopts cement kiln flue gas.
[0026] The present invention proposes for the first time to utilize the performance characteristics of lightweight aggregate and low-calcium cement, combined with the carbonation curing process to prepare carbonized lightweight aggregate concrete, effectively taking into account the comprehensive performance of the obtained lightweight concrete. During the carbonation and mineralization reaction of low-calcium cement, CO2 penetrates into the interior of the concrete through water as a medium, reacts with the carbonation active substances in the low-calcium cement, and produces carbonic acid and water. Due to its porous structural characteristics, lightweight aggregate absorbs and stores free water on the one hand, and "stores" part of CO2 in a CO2 environment on the other hand, acting as a reservoir and carbon source inside the concrete, continuously providing free water and CO2 for the hydration and carbonation reactions of low-calcium cement; at the same time, there are trace permeation channels in lightweight aggregate, which can serve as channels for the diffusion of water and CO2 inside the concrete; the free water slowly released from the trace channels of lightweight aggregate further promotes the self-curing of concrete; the CO2 gas diffused from the trace channels of lightweight aggregate ensures that the carbonization reaction inside the concrete is more efficient. The porous structure of lightweight aggregate promotes continuous hydration and carbonization reactions inside lightweight aggregate concrete, providing a continuous endogenous driving force for improving the performance of lightweight aggregate concrete.
[0027] Bio-based aggregate is a natural agricultural waste with the characteristics of light weight and high hardness. The present invention utilizes modified bio-based aggregate and low-calcium cement carbonization active mineral components to simultaneously carry out carbonization and mineralization. In addition, the admixture of the present invention uses naphthalene-based water reducer, and the carbonization enhancer uses polyglucosamine and polyethylene glycol. The above substances are beneficial to improving the absorption capacity of cement mineral components for CO2 and enhancing the degree of carbonization; in the process of coordinated carbonization, on the one hand, uncarbonized mineral components are attached to the surface of the modified bio-based aggregate, and the mineral components are secondary carbonized during the carbonization and curing process, and the generated carbonization products are attached to the surface of the aggregate to enhance the firmness of the aggregate. On the other hand, the nano to submicron CaCO3 particles generated by carbonization inside the concrete have a higher surface area. They act as induced crystal nuclei, stripping off hydration products on the surface of cement particles, inhibiting the formation of a protective layer of cement particles, accelerating the hydration process of low-calcium cement, and shortening the setting time of low-calcium cement. The carbonization products and hydration products of low-calcium cement, including calcium aluminate, calcium carbonate, and silica gel, jointly fill the pores inside the structure to improve the density of the concrete structure and reduce the shrinkage and deformation of the concrete. On the other hand, they "mesh" with the carbonization products and hydration products attached to the surface of the aggregate. The bite force between the products promotes the interweaving of the crystal structure to form a whole, making the transition zone at the interface between lightweight aggregate and cement stone denser, which is beneficial to improving the comprehensive performance of concrete.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] 1) The present invention is green and efficient, and is of great significance to the sustainable development of concrete. The present invention uses modified bio-based aggregate as lightweight aggregate. Bio-based aggregate is a natural agricultural waste, and its accumulation will cause harm to the environment. The present invention has the benefits of solid waste utilization and construction cost savings, reduces the industry's carbon footprint, and promotes the sustainable development of concrete; low-calcium cement is used to replace traditional silicate aluminate cement to prepare lightweight aggregate concrete, improving the current situation of high carbon emissions and high energy consumption in cement industry production; at the same time, CO2 in industrial waste gases such as cement kiln flue gas is used to cure lightweight aggregate concrete, further reducing CO2 emissions to the outside.
[0030] 2) Taking advantage of the carbonation activity of low-calcium cement, a dual carbonization mechanism is adopted to make the mineral components on the modified bio-based aggregate coating and the carbonation active components of low-calcium cement synergistically carbonize, and dual solidification absorbs CO2; on the one hand, carbonation mineralization accelerates the coagulation and hardening of low-calcium cement; on the other hand, the carbonization reaction prompts the carbonation products of the modified bio-based aggregate to "mesh" with the carbonation products of low-calcium cement, increasing the solid phase area, further enhancing the adhesion between aggregate and paste, and improving the density of the interface transition zone of lightweight concrete, with significant performance gains in lightweight concrete; the addition of carbonation enhancers not only increases the solidification and absorption of CO2, but also strengthens the biting force between carbonation products.
[0031] 3) Lightweight aggregate provides endogenous power for the carbonation and internal curing of low-calcium cement, ensuring the continuous improvement of the performance of lightweight aggregate concrete. The porous structure of lightweight aggregate enables it to act as a water reservoir and CO2 source inside the concrete. Through micro-channels, free water and CO2 continuously migrate into the cement paste, allowing the internal hydration and carbonation reactions to continue, comprehensively improving the performance of lightweight aggregate concrete. DETAILED DESCRIPTION
[0032] The following examples further illustrate the technical solution of the present invention, but are not intended to limit the scope of protection of the present invention.
[0033] A specific embodiment provides a method for preparing a modified bio-based aggregate, comprising the following steps:
[0034] (1) Soak the biomass raw materials in sodium hydroxide solution to remove surface oily impurities;
[0035] (2) Take it out and dry it, pour it into a crusher for crushing, and then use a screen to screen it;
[0036] (3) heat treating the screened biomass raw material to improve its surface structure;
[0037] (4) The heat-treated product is poured into a rotating drum container, and the interface modification slurry is added for roller coating. During the roller coating process, CO2 is continuously introduced. The surface of the modified bio-based aggregate has a 0.4-0.6 mm thick coating, and the surface material contains nano- to submicron-sized CaCO3 particles and unhydrated cement mineral components; the bulk density is ≤980 kg / m 3 , cylinder pressure strength ≥1.5MPa, 1h water absorption rate ≤18%.
[0038] Specifically, the biomass raw material is any one of oil palm shell, palm tree shell, coconut shell, peach shell or a mixture thereof; the age is 5-10 years, and the apparent density is 1330-1400 kg / m 3 .
[0039] Specifically, the concentration of the sodium hydroxide solution is 0.01% to 0.07%, the pH value is 10 to 13, and the soaking time is 12h to 24h.
[0040] Specifically, the particle sizes after sieving are 5-20 mm and 0-5 mm respectively.
[0041] Specifically, the heat treatment temperature is set to 60°C~80°C, and the time is 30min~40min.
[0042] Specifically, the interface modification slurry is mixed with concrete waste, water and dispersant; the mass ratio of water to concrete waste dry basis is (1-2): 1; the dispersant is polycarboxylate, and the dosage is 0.2%-0.4% of the total mass of the interface modification slurry;
[0043] The concrete waste is wastewater generated by cleaning concrete mixers, filter presses or concrete tankers, or waste slurry sediment generated by decomposition of waste concrete, and its dry basis components contain CaO 40-50wt%, SiO2 30~40wt%, and the rest are unavoidable impurities.
[0044] Specifically, the mass ratio of the interface modified slurry to the heat-treated product in the roller coating process is 1:(5~8); the rate of the roller coating process is 100rpm-200rpm, and the roller coating time is 1h~1.5h; the flow rate of the CO2 gas is 2~4L / min, and the concentration is 80~100vol%.
[0045] The specific embodiment also provides a carbonized lightweight aggregate concrete, which is composed of the following raw materials in parts by mass: 270-500 parts of low-calcium cement, 500-650 parts of coarse aggregate, 410-600 parts of fine aggregate, 140-180 parts of water, 5-10 parts of carbonization enhancer, and 5-10 parts of water reducer;
[0046] The coarse aggregate is one of modified bio-based aggregate, fly ash ceramsite, shale ceramsite, and expanded perlite, with a particle size of 5-20 mm; the fine aggregate is one of natural river sand, machine-made sand, and modified bio-based aggregate, with a fineness modulus of 2.3-3.2 and a crushing value of ≤25%.
[0047] Specifically, the low-calcium cement has C3S2, CS and C2S as main mineral phases, with C3S2 15-60%, CS 10-55%, C2S 20-60% by mass, and the sum of the mass proportions of the three mineral phases ≥ 87%, a calcium-silicon ratio of 1.4-1.7, a 45μm negative pressure sieve residue ≤ 26%, and a specific surface area ≥ 350m 2 / kg.
[0048] Specifically, the water reducer is a naphthalene-based water reducer, and its water reduction rate is 15-25%.
[0049] Specifically, the carbonization enhancer is one of polyglucosamine and polyethylene glycol; the molecular weight of the polyglucosamine is 150,000 to 400,000, and the molecular weight of the polyethylene glycol is 300 to 600; and the dosage is 0.5% to 1% of the total mass of the cementitious material.
[0050] The specific implementation also provides a method for preparing the above-mentioned carbonized lightweight aggregate concrete, comprising the following steps:
[0051] 1) Soak the coarse aggregate in water for 2 hours and then drain it, keeping the surface of the coarse aggregate saturated and dry;
[0052] 2) Mix with fine aggregate in proportion for 30 seconds and premix evenly; then add low-calcium cement and stir for 60 seconds until the mixture is evenly mixed; finally add water and admixtures and stir for 60-120 seconds to obtain a lightweight concrete mixture;
[0053] 3) Pour into a mold and cast into shape, then place in a CO2 curing environment for carbonization curing to obtain a carbonized lightweight aggregate concrete product.
[0054] Specifically, the carbonization curing system is: CO2 concentration 18-100 vol%, curing temperature 30-70°C, curing pressure 0.1-1.0 MPa, curing time 6-24 hours. The CO2 used in the carbonization curing step can be industrial waste gas such as cement kiln flue gas.
[0055] The admixture is naphthalene-based water reducer; the water reduction rate is 20%.
[0056] Example 1
[0057] A carbonized lightweight aggregate concrete, the preparation method of which comprises the following steps:
[0058] 1) Weigh the raw materials: 350 parts of low-calcium cement, 600 parts of coarse aggregate, 500 parts of machine-made sand, 160 parts of water, 5-10 parts of carbonation enhancer, and 5-10 parts of water reducer; the low-calcium cement is mainly composed of the following substances by mass fraction: C3S227%, C2S 33%, CS30%, calcium-silicon ratio of 1.51, 45μm negative pressure sieve residue of 15.2%, specific surface area of 373m 2 / kg; the carbonization enhancer is polyglucosamine with a molecular weight of 200,000; the coarse aggregate is shale ceramsite;
[0059] 2) Soak the ceramsite in water for 2 hours and then drain it, keeping the surface of the coarse aggregate saturated and dry;
[0060] 3) Stir the machine-made sand and soaked ceramsite for 30 seconds to make a uniform premix; then add low-calcium cement and stir for 60 seconds to make it uniform; add water, naphthalene-based water reducer and polyglucosamine and stir for 60-120 seconds to obtain a lightweight aggregate concrete mixture;
[0061] 4) Pour the concrete mixture into the mold, shape it, and vibrate and compact it;
[0062] 5) The obtained molded body is placed in a CO2 curing environment for carbonization curing to obtain a low-calcium lightweight concrete product, wherein the CO2 curing conditions adopted are: concentration 80%, temperature 50°C, carbonization pressure 0.3MPa, and carbonization time 12h.
[0063] Example 2
[0064] A method for preparing carbonized lightweight aggregate concrete is carried out according to the method in Example 1, except that the low-calcium cement used is different, wherein C3S231%, C2S 57%, CS 12%, the calcium-silicon ratio is 1.67, the 45μm negative pressure sieve residue is 10.2%, and the specific surface area is 442m 2 / kg.
[0065] Example 3
[0066] A method for preparing carbonized lightweight aggregate concrete is carried out according to the method in Example 1, except that the coarse aggregate used is modified bio-based aggregate.
[0067] Example 4
[0068] A method for preparing carbonized lightweight aggregate concrete is carried out according to the method in Example 3, except that the carbonization enhancer in the raw material is polyethylene glycol, model PEG-400, and molecular weight 400.
[0069] Example 5
[0070] A method for preparing carbonized lightweight aggregate concrete is carried out according to the method in Example 1, except that the carbonization system is 60% CO2 concentration, 40°C carbonization temperature, 0.5MPa carbonization pressure, and 24h carbonization time.
[0071] Comparative Example 1
[0072] A method for preparing carbonized lightweight aggregate concrete is carried out according to the method in Example 1, except that the low-calcium cement in the raw material is replaced by PO42.5 cement, the composition is C2S 21%, C3S 65%, C3A 1.3%, the calcium-silicon ratio is 2.8, the 45μm negative pressure sieve residue is 16.2%, and the specific surface area is 366m 2 / kg.
[0073] Comparative Example 2
[0074] A method for preparing carbonized lightweight aggregate concrete is carried out according to the method in Example 1, except that after the lightweight aggregate concrete is formed, it is cured in a standard protective room for 28 days at a temperature of 18-22° C. and a relative humidity of more than 95%.
[0075] Comparative Example 3
[0076] A method for preparing carbonized lightweight aggregate concrete is carried out according to the method in Example 1, except that there is no carbonization enhancer in the lightweight concrete raw materials.
[0077] Comparative Example 4
[0078] A method for preparing carbonized lightweight aggregate concrete is carried out according to the method in Example 1, except that the shale ceramsite used has no water soaking process.
[0079] Carbonized lightweight aggregate concrete prepared in Examples 1 to 5 and Comparative Examples 1 to 4 was tested for performance according to GB / T50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete" and JGJ / T12-2019 "Technical Standard for Application of Lightweight Aggregate Concrete". The results are shown in Table 1.
[0080] Table 1
[0081] serial number 28d compressive strength / MPa <![CDATA[Dry apparent density / kg / m 3 > 28d shrinkage value / mm / m Example 1 28.2 1480 0.31 Example 2 25.0 1550 0.34 Example 3 31.2 1520 0.29 Example 4 23.1 1490 0.30 Example 5 30.1 1550 0.32 Comparative Example 1 20.3 1500 0.37 Comparative Example 2 12.8 1730 0.42 Comparative Example 3 21.2 1450 0.33 Comparative Example 4 10.2 1630 0.52
[0082] It can be seen from Table 1 that:
[0083] Combining Comparative Example 1 with Examples 1-5 and Table 1, it can be seen that the 28d compressive strength of Comparative Example 1 is significantly lower than that of Examples 1-5, and the 28d shrinkage value of Comparative Example 1 is greater than that of Examples 1-5. This is because ordinary silicates have high hydration activity and low carbonization activity, and carbonization curing cannot enhance the meshing force of carbonization products, the interface transition zone cannot be improved, and the performance of lightweight aggregate concrete is average.
[0084] Combining Comparative Example 2 with Examples 1-5 and Table 1, it can be seen that the 28d compressive strength of Comparative Example 2 is less than that of Examples 1-5, and the 28d shrinkage value is greater than that of Examples 1-5, indicating that carbonation curing can stimulate the high carbonization activity of low-calcium cement, strengthen the meshing effect between low-calcium cement and aggregate, and improve the performance of lightweight aggregate concrete.
[0085] Combining Comparative Example 3 with Examples 1-5 and Table 1, it can be seen that the 28d compressive strength of Comparative Example 3 is less than that of Examples 1-5, indicating that the carbonization enhancer promotes the carbonization reaction of low-calcium cement, further improves the carbonization mineralization degree of lightweight aggregate concrete, and improves the performance of concrete.
[0086] Combining Comparative Example 4 with Examples 1-5 and Table 1, it can be seen that the 28d compressive strength of Comparative Example 4 is less than that of Examples 1-5, and the 28d shrinkage value is greater than that of Examples 1-5, indicating that the pre-immersion treatment of ceramsite can improve the strength of lightweight aggregate concrete. Ceramsite provides free water inside the concrete, which continuously promotes the hydration and carbonization reaction.
[0087] By comparing Example 3 with Example 1 and combining with Table 1, it can be seen that the 28d compressive strength of Example 3 is close to that of Example 1, indicating that the performance of the modified bio-based aggregate as an aggregate filler is comparable to that of lightweight aggregate concrete prepared from ceramsite.
[0088] The above results show that the carbonized lightweight aggregate concrete prepared in Examples 1 to 5 has high compressive strength and low shrinkage; based on the characteristics of low hydration activity and carbonization activity of low-calcium cement, by recycling solid waste in industrial production and combining a simple and easy-to-control carbonization curing process, the good mechanical properties and long-term properties of the obtained lightweight aggregate concrete can be effectively taken into account, which has important economic and environmental benefits.
[0089] The above embodiments are only examples for clear explanation, and are not intended to limit the implementation methods. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here, so the obvious changes or modifications derived are still within the protection scope of the invention.
Claims
1. A carbonized lightweight aggregate concrete, characterized in that It is composed of the following raw materials in parts by mass: 270-500 parts of low-calcium cement, 500-650 parts of coarse aggregate, 410-600 parts of fine aggregate, 140-180 parts of water, 5-10 parts of carbonation enhancer, and 5-10 parts of water reducer; The low-calcium cement has C3S2, CS and C2S as main mineral phases, with C3S2 15-60% by mass, CS 10-55% by mass, C2S 20-60% by mass, and the sum of the mass proportions of the three mineral phases ≥87%, a calcium-silicon ratio of 1.4-1.7, a 45μm negative pressure sieve residue ≤26%, and a specific surface area ≥350m 2 / kg; The coarse aggregate is one of modified bio-based aggregate, fly ash ceramsite, shale ceramsite, and expanded perlite, and has a particle size of 5-20 mm; before preparing the carbonized lightweight aggregate concrete, the coarse aggregate is soaked in water for 2 hours and then drained to keep the saturated surface of the coarse aggregate dry; The fine aggregate is a modified bio-based aggregate with a fineness modulus of 2.3 to 3.2 and a crushing value of ≤25%; The modified bio-based aggregate is prepared in the following manner: The biomass raw materials are soaked in a sodium hydroxide solution to remove surface oily impurities; After taking out, crush, sieve and dry, heat treat at 60℃~80℃ for 30min~40min; Add interface modification slurry for roll coating, and continuously introduce CO2 during the roll coating process; Wherein, the biomass raw material includes any one of peach shell, palm tree shell, coconut shell or a mixture thereof; The interface modification slurry is prepared by mixing concrete waste, water and dispersant; the mass ratio of water to concrete waste dry basis (1-2): 1; the dispersant is polycarboxylate, and the dosage is 0.2%-0.4% of the total mass of the interface modification slurry; The concrete waste is wastewater generated by cleaning concrete mixers, filter presses or concrete tankers, or waste slurry sediment generated by decomposition of waste concrete, and its dry basis composition contains CaO 40-50wt%, SiO2 30~40wt%, and the rest are unavoidable impurities.
2. Carbonized lightweight aggregate concrete according to claim 1, characterized in that The water reducing agent is a naphthalene-based water reducing agent, and its water reducing rate is 15-25%.
3. Carbonized lightweight aggregate concrete according to claim 1, characterized in that The carbonization enhancer is one of polyglucosamine and polyethylene glycol; the molecular weight of the polyglucosamine is 150,000 to 400,000, and the molecular weight of the polyethylene glycol is 300 to 600.
4. The method for preparing the carbonized lightweight aggregate concrete according to claim 1, characterized in that The following steps are involved: 1) Soak the coarse aggregate in water for 2 hours and then drain it, keeping the surface of the coarse aggregate saturated and dry; 2) Mix with fine aggregate in proportion for 30 seconds and premix evenly; then add low-calcium cement and stir for 60 seconds until the mixture is evenly mixed; finally add water and admixtures and stir for 60-120 seconds to obtain a lightweight concrete mixture; 3) Pour into a mold for casting and forming, place in a CO2 curing environment for carbonization curing, and obtain a carbonized lightweight aggregate concrete product.
5. The method for preparing carbonized lightweight aggregate concrete according to claim 4, characterized in that The carbonization curing system is as follows: CO2 concentration 18-100 vol%, curing temperature 30-70°C, curing pressure 0.1-1.0 MPa, and curing time 6-24 h.
6. The method for preparing carbonized lightweight aggregate concrete according to claim 4, characterized in that The CO2 curing environment adopts cement kiln flue gas.