A high-resistance target material with low bulk resistivity and a preparation method thereof

Through the mixed ball milling method of indium oxide, zirconia and silicon oxide and spray granulation process, the problem of high resistivity of traditional high-resistance targets is solved, and a high-resistance target with low body resistivity is prepared, suitable for microelectronics and optoelectronic devices improve the efficiency and reliability of the device.

CN116835965BActive Publication Date: 2024-12-03WUHU YINGRI TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310740853.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-21
Publication Date
2024-12-03
Estimated Expiration
2043-06-21

AI Technical Summary

Technical Problem

The body resistivity of traditional high-resistance targets is high, which leads to a larger voltage required when preparing semiconductor films, resulting in reduced device efficiency and reliability, and easily lead to impurities and defects in the film.

Method used

A mixed ball milling method of indium oxide, zirconia and silicon oxide is used, and a two-step ball milling and spray granulation process is used to add coarse silica particles and polyvinyl alcohol solution to form a high-resistance target material with low volume resistivity.

Benefits of technology

The prepared high-resistance target has high relative density, small grain size and low resistivity. It is suitable for microelectronics and optoelectronic devices, improving the efficiency and reliability of the device and reducing the body resistivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116835965B_ABST
    Figure CN116835965B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of target material technology, and in particular to a high-resistance target material with low volume resistivity and a preparation method thereof. The preparation method of the high-resistance target material with low volume resistivity of the present invention comprises the following steps: (1) selection of raw materials, (2) primary ball milling, (3) secondary ball milling, (4) fat doping, (5) spray granulation, (6) primary molding, (7) secondary molding, and (8) high-temperature sintering. The high-resistance target material with low volume resistivity of the present invention has a relative density of not less than 99.1%, a grain size of not more than 10um, and a resistivity of not more than 0.23mΩ.cm. The high-resistance target material prepared by the method of the present invention can be widely used in the fields of microelectronics, optoelectronic devices, etc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of target materials, and in particular to a high-resistance target material with low volume resistivity and a preparation method thereof. Background Art

[0002] High-resistance targets are very important materials in the semiconductor industry. Liquid crystal displays are one of the important application scenarios of high-resistance targets, where high-resistance targets are mainly used in the manufacture of shielding layers. Since the shielding layer needs to have high uniformity and high resistance characteristics, the properties of high-resistance targets directly affect the performance and quality of liquid crystal displays.

[0003] At present, the main components of high-resistance targets are indium oxide, zirconium oxide, silicon oxide or indium oxide, tin oxide, and silicon oxide. The three powders are mixed by mechanical mixing, granulated, and then shaped and sintered to prepare high-resistance targets. However, the high resistivity of traditional high-resistance targets will result in a higher voltage required to maintain the required number of ejected ions when preparing semiconductor films, which will lead to lower device efficiency and instability. In addition, higher resistivity can easily cause impurities and defects in the film, thereby reducing the efficiency and reliability of the device. Summary of the invention

[0004] In view of this, an object of the present invention is to provide a high-resistance target material with low volume resistivity and a preparation method thereof, so as to solve the problem of high volume resistivity of conventional high-resistance target materials.

[0005] Based on the above purpose, the present invention provides a method for preparing a high-resistance target material with low volume resistivity, and the specific preparation steps are as follows:

[0006] (1) Selection of raw materials: Indium oxide particle size D50 is 0.3-0.8um, purity is not less than 99.99%, zirconium oxide particle size D50 is 0.5-1.5um, purity is not less than 99.5%, silicon oxide particle size D50 is 20-30um, purity is not less than 99.9%;

[0007] (2) Primary ball milling: Add indium oxide, zirconium oxide and pure water into a ball mill filled with φ1-2 mm zirconium beads, and ball mill for 36-48 hours to obtain a mixed slurry;

[0008] (3) Secondary ball milling: Add silicon oxide to the mixed slurry and ball mill for 2-5 hours to obtain a high-resistance mixed slurry;

[0009] (4) Fat doping: Add 5%-8% polyvinyl alcohol solution by mass into the high-resistance mixed slurry, and ball mill for 10-20 minutes to obtain a fat-doped high-resistance mixed slurry;

[0010] (5) Spray granulation: The lipid-doped high-resistance mixed slurry is granulated in a centrifugal spray granulator with an inlet air temperature of 200-230°C and an outlet air temperature of 80-100°C to obtain a high-resistance powder;

[0011] (6) One-step molding: The high-resistance powder is loaded into a flat target molding mold for one-step pre-compression molding at a molding pressure of 200-500 Kgf / cm 2 , the holding time is 5-20min, and a green embryo is obtained;

[0012] (7) Secondary molding: The primary blank is placed in a flexible latex bag, vacuumed, and then placed in an isostatic press for secondary molding at a molding pressure of 250-300 MPa and a holding time of 30-60 min to obtain a secondary blank;

[0013] (8) High temperature sintering: The secondary green blank is placed in a high temperature sintering furnace in a normal pressure oxygen atmosphere for sintering at a temperature of 1500°C for 25-30 hours to obtain a high resistance target material with low bulk resistivity.

[0014] Preferably, the content of the raw materials in step (1) is: 5%-10% by mass of zirconium oxide, 5%-15% by mass of silicon oxide, and the balance is indium oxide.

[0015] Preferably, the amount of pure water added in step (2) is equal to the mixed weight of indium oxide and zirconium oxide.

[0016] Preferably, the amount of polyvinyl alcohol added in step (4) is 1-3% of the weight of the high-resistance mixed slurry.

[0017] Preferably, in step (5), the particle size D50 of the high-resistance powder is 35-50 um.

[0018] Preferably, in step (8), the relative density of the high-resistance target material with low bulk resistivity is not less than 99.1%, the grain size is not greater than 10 um, and the resistivity is not greater than 0.23 mΩ.cm.

[0019] Beneficial effects of the present invention:

[0020] The present invention provides a method for preparing a high-resistance target material with low bulk resistivity, using coarse silicon oxide powder with a particle size of not less than 20 μm and a two-step ball milling method. First, indium oxide and zirconium oxide are ball milled, and then silicon oxide is added for secondary ball milling. In the preparation process, coarse silicon oxide particles are used and silicon oxide is added at the end to complete the two-step ball milling process in a short time. By this method, the non-conductive phase In in the microstructure of the prepared high-resistance target material is 2 (Si 2 O 7) are unevenly distributed to form “islands”, which is beneficial to reducing the bulk resistivity of the target material.

[0021] The present invention provides a high-resistance target material with low bulk resistivity, a relative density of not less than 99.1%, a grain size of not more than 10um, a resistivity of not more than 0.23mΩ.cm, uniform color, and no color difference, and has wide application value in the fields of microelectronics and optoelectronic devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required to be used in the embodiments or the description of the prior art are briefly introduced below.

[0023] Figure 1 This is an enlarged picture of the high-resistance powder in Example 2 of the present invention;

[0024] Figure 2 This is a grain picture of the high-resistance target material with low bulk resistivity in Example 2 of the present invention (after acid corrosion). DETAILED DESCRIPTION

[0025] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.

[0026] Example 1

[0027] A method for preparing a high-resistance target material with low volume resistivity, the specific preparation steps are as follows:

[0028] (1) Selection of raw materials: Indium oxide particle size D50 is 0.4um, purity is 99.992%, zirconium oxide particle size D50 is 0.7um, purity is 99.51%, silicon oxide particle size D50 is 22um, purity is 99.93%;

[0029] (2) Primary ball milling: 80 g of indium oxide, 5 g of zirconium oxide and 85 g of pure water were added to a ball mill filled with φ2 mm zirconium beads and ball milled for 36 h to obtain a mixed slurry;

[0030] (3) Secondary ball milling: Add 15 g of silicon oxide to the mixed slurry and ball mill for 2 h to obtain a high-resistance mixed slurry;

[0031] (4) Fat doping: Add 2 g of 5%-8% polyvinyl alcohol solution to the high-resistance mixed slurry and ball mill for 10-20 min to obtain a fat-doped high-resistance mixed slurry;

[0032] (5) Spray granulation: The lipid-doped high-resistance mixed slurry is granulated in a centrifugal spray granulator with an inlet air temperature of 200°C and an outlet air temperature of 80°C to obtain a high-resistance powder;

[0033] (6) One-step molding: The high-resistance powder is loaded into a flat target molding mold for one-step pre-compression molding at a molding pressure of 200 Kgf / cm 2 , the holding time is 20 minutes, and a green embryo is obtained;

[0034] (7) Secondary molding: The primary blank is placed in a flexible latex bag, vacuumed, and then placed in an isostatic press for secondary molding at a molding pressure of 250 MPa and a holding time of 60 min to obtain a secondary blank;

[0035] (8) High-temperature sintering: The secondary green blank is placed in a high-temperature sintering furnace in a normal-pressure oxygen atmosphere for sintering at a temperature of 1500°C for 25 hours to obtain a high-resistance target material with low bulk resistivity.

[0036] Example 2

[0037] A method for preparing a high-resistance target material with low volume resistivity, the specific preparation steps are as follows:

[0038] (1) Selection of raw materials: Indium oxide particle size D50 is 0.6um, purity is 99.991%, zirconium oxide particle size D50 is 1.1um, purity is 99.53%, silicon oxide particle size D50 is 22um, purity is 99.93%;

[0039] (2) Primary ball milling: 83 g of indium oxide, 7 g of zirconium oxide and 100 g of pure water were added to a ball mill filled with φ2 mm zirconium beads and ball milled for 42 h to obtain a mixed slurry;

[0040] (3) Secondary ball milling: Add 10 g of silicon oxide to the mixed slurry and ball mill for 3.5 h to obtain a high-resistance mixed slurry;

[0041] (4) Fat doping: Add 2 g of 5% polyvinyl alcohol solution into the high-resistance mixed slurry and ball mill for 15 min to obtain a fat-doped high-resistance mixed slurry;

[0042] (5) Spray granulation: The lipid-doped high-resistance mixed slurry is granulated in a centrifugal spray granulator with an inlet air temperature of 215°C and an outlet air temperature of 90°C to obtain a high-resistance powder;

[0043] (6) One-step molding: The high-resistance powder is loaded into the flat target molding mold for one-step pre-compression molding at a molding pressure of 350 Kgf / cm 2 , the holding time is 15 minutes, and a green embryo is obtained;

[0044] (7) Secondary molding: The primary blank is placed in a flexible latex bag, vacuumed, and then placed in an isostatic press for secondary molding at a molding pressure of 275 MPa and a holding time of 45 min to obtain a secondary blank;

[0045] (8) High-temperature sintering: The secondary green blank is placed in a high-temperature sintering furnace in a normal-pressure oxygen atmosphere for sintering at a temperature of 1500°C for 27 hours to obtain a high-resistance target material with low bulk resistivity.

[0046] Example 3

[0047] A method for preparing a high-resistance target material with low volume resistivity, the specific preparation steps are as follows:

[0048] (1) Selection of raw materials: Indium oxide particle size D50 is 0.7um, purity is 99.991%, zirconium oxide particle size D50 is 1.3um, purity is 99.6%, silicon oxide particle size D50 is 28um, purity is 99.92%;

[0049] (2) Primary ball milling: 85 g of indium oxide, 10 g of zirconium oxide and 95 g of pure water were added to a ball mill filled with φ2 mm zirconium beads and ball milled for 48 h to obtain a mixed slurry;

[0050] (3) Secondary ball milling: Add 5 g of silicon oxide to the mixed slurry and ball mill for 5 h to obtain a high-resistance mixed slurry;

[0051] (4) Fat doping: Add 2 g of 8% polyvinyl alcohol solution into the high-resistance mixed slurry and ball mill for 20 min to obtain a fat-doped high-resistance mixed slurry;

[0052] (5) Spray granulation: The lipid-doped high-resistance mixed slurry is granulated in a centrifugal spray granulator with an inlet air temperature of 230°C and an outlet air temperature of 80°C to obtain a high-resistance powder;

[0053] (6) One-step molding: The high-resistance powder is loaded into a flat target molding mold for one-step pre-compression molding at a molding pressure of 500 Kgf / cm 2 , the holding time is 5 minutes, and a green embryo is obtained;

[0054] (7) Secondary molding: The primary blank is placed in a flexible latex bag, vacuumed, and then placed in an isostatic press for secondary molding at a molding pressure of 300 MPa and a holding time of 30 min to obtain a secondary blank;

[0055] (8) High-temperature sintering: The secondary green blank is placed in a high-temperature sintering furnace in a normal-pressure oxygen atmosphere for sintering at a temperature of 1500°C for 30 hours to obtain a high-resistance target material with low bulk resistivity.

[0056] Comparative Example 1

[0057] A method for preparing a high-resistance target material, the specific preparation steps are as follows:

[0058] (1) Selection of raw materials: Indium oxide particle size D50 is 0.6 μm, purity is 99.991%, zirconium oxide particle size D50 is 1.1 μm, purity is 99.53%, silicon oxide particle size D50 is 1 μm, purity is 99.93%;

[0059] The remaining steps are the same as in Example 2.

[0060] Comparative Example 2

[0061] A method for preparing a high-resistance target material, the specific preparation steps are as follows:

[0062] (1) Selection of raw materials: Indium oxide particle size D50 is 0.6um, purity is 99.991%, zirconium oxide particle size D50 is 1.1um, purity is 99.53%, silicon oxide particle size D50 is 22um, purity is 99.93%;

[0063] (2) Primary ball milling: 83 g of indium oxide, 7 g of zirconium oxide, 10 g of silicon oxide and 100 g of pure water were added to a ball mill filled with φ2 mm zirconium beads and ball milled for 42 h to obtain a mixed slurry;

[0064] The remaining steps are the same as in Example 2.

[0065] Comparative Example 3

[0066] A method for preparing a high-resistance target material, the specific preparation steps are as follows:

[0067] (1) Selection of raw materials: Indium oxide particle size D50 is 0.6 μm, purity is 99.991%, zirconium oxide particle size D50 is 1.1 μm, purity is 99.53%, silicon oxide particle size D50 is 1 μm, purity is 99.93%;

[0068] (2) Primary ball milling: Add 83 g of indium oxide, 7 g of zirconium oxide, 10 g of silicon oxide and 100 g of pure water into a ball mill filled with φ2 mm zirconium beads and ball mill for 42 h to obtain a high-resistance mixed slurry;

[0069] The remaining steps are the same as in Example 2.

[0070] Comparative Example 4

[0071] A method for preparing a high-resistance target material, the specific preparation steps are as follows:

[0072] (1) Selection of raw materials: Indium oxide particle size D50 is 0.6um, purity is 99.991%, zirconium oxide particle size D50 is 1.1um, purity is 99.53%, silicon oxide particle size D50 is 22um, purity is 99.93%;

[0073] (2) Primary ball milling: 83 g of indium oxide, 7 g of zirconium oxide and 100 g of pure water were added to a ball mill filled with φ2 mm zirconium beads and ball milled for 42 h to obtain a mixed slurry;

[0074] (3) Secondary ball milling: Add 10 g of silicon oxide to the mixed slurry and ball mill for 20 h to obtain a high-resistance mixed slurry;

[0075] The remaining steps are the same as in Example 2.

[0076] Performance test: The relative density and volume resistivity of the target materials prepared in Examples 1-3 and Comparative Examples 1-4 were tested. The test results are shown in Table 1.

[0077] Table 1 Performance test results of the targets prepared in Examples 1-3 and Comparative Examples 1-4

[0078]

[0079] Data analysis: It can be seen from Examples 1-3 that the relative density of the high-resistance target material with low volume resistivity prepared by the present invention is not less than 99.1%, and the resistivity is not greater than 0.23 mΩ.cm. Figure 1 It can be seen that the high-resistance powder prepared by the present invention contains large-size particles, and the particle size D50 is 42 μm. Figure 2 It can be seen that the grain size prepared by the present invention is not greater than 10um, and an "island" structure is generated, which helps to reduce the bulk resistivity of the target material. It can be seen from Example 2 and Comparative Examples 1-4 that the coarse silicon oxide powder, the two-step ball milling method and the secondary short-time ball milling jointly promote the reduction of the bulk resistivity of the target material.

[0080] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention (including the claims) is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.

[0081] The present invention is intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing a high-resistance target material with low bulk resistivity, characterized in that: The specific preparation steps are as follows: (1) Selection of raw materials: Indium oxide particle size D50 is 0.3-0.8um, purity is not less than 99.99%, zirconium oxide particle size D50 is 0.5-1.5um, purity is not less than 99.5%, silicon oxide particle size D50 is 20-30um, purity is not less than 99.9%; (2) Primary ball milling: Add indium oxide, zirconium oxide and pure water into a ball mill filled with φ1-2 mm zirconium beads and ball mill for 36-48 hours to obtain a mixed slurry; (3) Secondary ball milling: Add silicon oxide to the mixed slurry and ball mill for 2-5 hours to obtain a high-resistance mixed slurry; (4) Fat doping: Add 5%-8% polyvinyl alcohol solution by mass into the high-resistance mixed slurry, and ball mill for 10-20 minutes to obtain a fat-doped high-resistance mixed slurry; (5) Spray granulation: The lipid-doped high-resistance mixed slurry is granulated in a centrifugal spray granulator with an inlet air temperature of 200-230°C and an outlet air temperature of 80-100°C to obtain a high-resistance powder; (6) One-step molding: The high-resistance powder is loaded into a flat target molding mold for one-step pre-compression molding. The molding pressure is 200-500Kgf / cm 2 , the holding time is 5-20min, and a green embryo is obtained; (7) Secondary molding: The primary blank is placed in a flexible latex bag, vacuumed, and then placed in an isostatic press for secondary molding at a molding pressure of 250-300 MPa and a holding time of 30-60 min to obtain a secondary blank; (8) High temperature sintering: The secondary green blank is placed in a high temperature sintering furnace in a normal pressure oxygen atmosphere for sintering at a temperature of 1500°C for a holding time of 25-30 hours to obtain a high resistance target material with low bulk resistivity; In step (5), the particle size D50 of the high-resistance powder is 35-50 μm; In the step (8), the relative density of the high-resistance target material with low bulk resistivity is not less than 99.1%, the grain size is not greater than 10 um, and the resistivity is not greater than 0.23 mΩ.cm.

2. The method for preparing a high-resistance target material with low volume resistivity according to claim 1, characterized in that: The content of the raw materials in step (1) is: 5%-10% by weight of zirconium oxide, 5%-15% by weight of silicon oxide, and the balance of indium oxide.

3. The method for preparing a high-resistance target material with low volume resistivity according to claim 1, characterized in that: The amount of pure water added in step (2) is equal to the mixed weight of indium oxide and zirconium oxide.

4. The method for preparing a high-resistance target material with low volume resistivity according to claim 1, characterized in that: The amount of polyvinyl alcohol added in step (4) is 1-3% of the weight of the high-resistance mixed slurry.