A positive electrode material and its preparation method and application
By using glass-like material contained in phosphorus elements to coat the positive electrode active material to form a uniform cladding layer, the problem of poor circulation and storage performance of the lithium-ion battery positive electrode material under high voltage is solved, and the electrochemical performance of the battery is significantly improved and security.
Patent Information
- Application Number
- CN202310942864.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-28
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-07-28
AI Technical Summary
The existing lithium-ion battery positive electrode materials have poor circulation and storage performance at high voltages, and have poor high temperature performance, making it difficult to form a uniform and complete cladding layer to isolate the electrolyte, resulting in serious Mn dissolution and side reactions.
Using glass-like phase materials as the cladding layer, a firm, uniform and stable cladding layer is formed by defining the specific surface area difference before and after cladding, and a cladding layer containing phosphorus elements is used to improve the cycle stability and storage of the positive electrode material. performance.
It significantly improves the cycling stability and storage performance of the positive electrode material at high voltage, reduces electrolyte decomposition and surface ion dissolution, and improves the cycling performance, capacity retention and safety performance of the battery.
Smart Images

Figure CN116845213B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to a positive electrode material and a preparation method and application thereof. Background Art
[0002] The positive electrode material is a key factor in determining the performance of lithium-ion batteries. 2 Layered materials represented by ternary NCM, LiFePO 4 Olivine-type materials represented by LiMn 2 O 4 Spinel materials represented by LiCoO 2 and ternary NCM have high energy density and good cycle performance but are expensive; LiFePO 4 The cycle performance is excellent, the safety is good and the price is low, but the energy density is low, and the actual capacity is close to the theoretical capacity, so it is difficult to increase significantly; LiMn 2 O 4 The structure is stable, but the capacity is low and the Mn dissolution problem is serious. The high-temperature performance is poor and there are few practical application scenarios.
[0003] LiNi 0.5 Mn 1.5 O 4 (Lithium Nickel Manganese Oxide) is LiMn 2 O 4 Developed on the basis of Ni 2+ The addition of Mn 3+ Up to Mn 4+ The valence of Mn is greatly improved. 2 O 4 The specific capacity is similar (about 146.7mAh / g), but the working voltage of lithium nickel manganese oxide (4.75V) is higher than that of LiMn 2 O 4 The operating voltage (4V) is about 19% higher and has a higher energy density. 2 , NCM and LiFePO 4 The energy density of lithium nickel manganese oxide is improved mainly by increasing the voltage rather than by adding additional Li as in lithium-rich layered materials, thus greatly reducing the watt-hour cost and having a very high cost-performance ratio. However, the higher voltage makes the interface problem of lithium nickel manganese oxide particularly prominent. Electrolyte oxidation, interface side reactions, changes in the interface layer structure, etc. lead to poor cycle performance, high temperature performance and storage performance of lithium nickel manganese oxide as the positive electrode, and serious gas production.
[0004] In the related art, most of the coating materials are usually coated on the surface of lithium nickel manganese oxide to improve the electrochemical performance of the battery. However, most of the coating materials are often in the form of granular materials, with many and small particles, and are coated in islands on the outer surface of lithium nickel manganese oxide. In addition, there is often partial aggregation between the coating materials, making it difficult to form a uniform and complete package, and it is impossible to isolate the contact between lithium nickel manganese oxide and the electrolyte. At present, there are also conductive glass used for surface coating. For example, patent document CN116014142A discloses the use of lithium ion conductive glass Li 2 OB 2 O 3 -M is used to coat lithium nickel manganese oxide, and patent document CN102867949B uses lithium borosilicate glass to coat the positive electrode active material. However, the high-voltage stability of the boron element in the above-mentioned coating material is poor, which is not suitable for the high-voltage lithium nickel manganese oxide system, and the degree of improvement in electrochemical performance under high voltage is far from meeting the requirements. Summary of the invention
[0005] The present invention provides a positive electrode material. By limiting the material of the coating layer and the difference in specific surface area before and after coating, a firm, uniform and stable coating layer is ensured, which is beneficial to improving the cycle stability and storage performance of the positive electrode material under high voltage. The positive electrode material is applied to a battery, which is beneficial to improving the electrochemical performance of the battery.
[0006] The present invention also provides a method for preparing a positive electrode material, which can produce the above-mentioned positive electrode material with excellent performance. Applying the positive electrode material to a battery is beneficial to improving the cycle performance, capacity retention rate and safety performance of the battery.
[0007] The present invention also provides a positive electrode sheet. Since the positive electrode sheet includes the positive electrode material, the positive electrode sheet is applied to a battery, which is beneficial to improving the cycle performance, capacity retention rate and safety performance of the battery.
[0008] The present invention also provides a battery, which comprises the positive electrode sheet and has excellent cycle performance, capacity retention rate and safety performance.
[0009] In a first aspect of the present invention, there is provided a positive electrode material, comprising a positive electrode active material and a coating layer coated on the surface of the positive electrode active material, wherein the coating layer material is a glass-like phase material, and the coating layer material contains phosphorus;
[0010] The specific surface area reduction rate of the positive electrode active material after being coated by the coating layer is ≥5%.
[0011] The positive electrode material as described above, wherein the softening point of the glass-like phase material is ≤1000° C.; and / or,
[0012] The voltage window of the positive electrode material is 3.5-4.95V.
[0013] The positive electrode material as described above, wherein the glass-like phase material comprises the following components by weight percentage: 40-90% of phosphorus pentoxide, 10-60% of oxide containing element A, and 0-10% of alkali metal oxide; wherein,
[0014] The A element includes at least one of Si, Ce, Be, Te, Ta, Al, Cu, Nb, V, W, Sr, Mg, Ti, La, Ca, Zn, Sb, Se, and I.
[0015] The positive electrode material as described above, wherein the oxide containing the A element includes Be 2 O 3 , MgO, CaO, SrO, TiO 2 、V 2 O 5 CrO 3 、Co 3 O 4 、NiO、CuO、ZnO、ZrO 2 , Nb 2 O 5 、MoO 3 , WO 3 、 2 O 5 ,La 2 O 3 、CeO 2 、Nd 2 O 3 、Al 2 O 3 SnO 2 、SiO 2 , Sb 2 O 5 、TeO 2 , SeO 2 ,I 2 O 5 At least one of; and / or,
[0016] The alkali metal oxides include K 2 O. Li 2 O、Na 2 At least one of O.
[0017] The positive electrode material as described above, wherein the mass of the coating layer is 0.1 to 10 wt % of the mass of the positive electrode active material.
[0018] The positive electrode material as described above, wherein the chemical formula of the positive electrode active material is Li 1+x Ni 0.5+y Mn 1.5+z Mu O w , where -0.1≤x≤0.3, -0.2≤y≤0.2, -0.2≤z≤0.2, 0≤u≤0.2, 3.8≤w≤4.3;
[0019] Among them, M includes at least one of Mg, Al, Ca, Sc, Ti, V, Cr, Fe, Co, Cu, Zn, Ga, Sr, Y, Zr, Nb, Mo, Ru, Ta, W, B, Si, Ge, Sb, Te, P, S, and F.
[0020] The positive electrode material as described above, wherein the positive electrode active material is a single crystal material, and the particle size of the single crystal material is 0.5 to 30 μm; or
[0021] The positive electrode active material is a polycrystalline material, and the particle size of the polycrystalline material is 0.1 to 20 μm.
[0022] A second aspect of the present invention provides a method for preparing the positive electrode material according to the first aspect, comprising the following steps:
[0023] The positive electrode active material is mixed with a glass-like phase material, and after a first sintering treatment and an annealing treatment, the positive electrode material is obtained; wherein the temperature of the first sintering treatment is 700-1000°C, and the time is 1-30 hours; the temperature of the annealing treatment is 400-800°C, and the time is 1-20 hours.
[0024] The preparation method as described above, wherein the glass-like phase material is prepared by a method comprising the following process: uniformly mixing a P compound, a compound containing an A element, and an alkali metal compound according to a mass ratio to obtain a mixture;
[0025] The glass-like phase material is obtained by melting and crushing the mixed material; wherein the temperature of the melting treatment is 800 to 1300° C. and the time is 3 to 10 hours.
[0026] In the preparation method as described above, the P compound is phosphorus pentoxide, or at least one of compounds that can form phosphorus pentoxide after sintering in air or an oxidizing atmosphere, preferably at least one of phosphoric acid, ammonium monohydrogen phosphate, ammonium dihydrogen phosphate, and diammonium hydrogen phosphate;
[0027] The compound containing element A is an oxide containing element A, or at least one of compounds containing element A oxide that can be formed after sintering in air or an oxidizing atmosphere;
[0028] The alkali metal compound is an alkali metal oxide, or at least one compound that can form an alkali metal oxide after sintering in air or an oxidizing atmosphere.
[0029] In the preparation method as described above, the alkali metal compound includes at least one of phosphorus pentoxide, lithium carbonate, lithium hydroxide, lithium oxalate, lithium acetate, lithium citrate, lithium fluoride and sodium carbonate.
[0030] According to a third aspect of the present invention, a positive electrode sheet is provided, wherein the positive electrode sheet comprises the positive electrode material described in the first aspect or the positive electrode material prepared by the preparation method described in the second aspect.
[0031] A fourth aspect of the present invention provides a lithium-ion battery, wherein the lithium-ion battery comprises the positive electrode sheet described in the third aspect.
[0032] The implementation of the present invention has at least the following beneficial effects:
[0033] The positive electrode material provided by the present invention utilizes the uniformity of the glass-like phase material and its fluidity at high temperature, and at the same time, by limiting the difference in specific surface area before and after coating, the glass-like phase material is firmly, uniformly and completely coated on the surface of the positive electrode active material to form a protective coating layer, thereby improving the cycle stability and storage performance of the positive electrode material under high voltage. The positive electrode material is applied to the battery, which can fully isolate the contact between the electrolyte and the positive electrode active material, reduce the decomposition of the electrolyte under high voltage and the occurrence of surface side reactions, reduce the dissolution of surface ions, and effectively improve the stability of the positive electrode material, thereby improving the cycle performance, capacity retention rate and safety performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 is a SEM image of the positive electrode material A1 of Comparative Example 1 of the present invention at the first magnification;
[0035] Figure 2 is a SEM image of the positive electrode material A1 of Comparative Example 1 of the present invention at the second magnification;
[0036] Figure 3 is a SEM image of the positive electrode material C1 of Example 1 of the present invention at a first magnification;
[0037] Figure 4 is a SEM image of the positive electrode material C1 of Example 1 of the present invention at the second magnification;
[0038] Figure 5 is a SEM image of the positive electrode material C7 of Example 7 of the present invention at a first magnification;
[0039] Figure 6 is a SEM image of the positive electrode material C7 of Example 7 of the present invention at the second magnification;
[0040] Figure 7is a SEM image of the positive electrode material C17 of Comparative Example 7 of the present invention at the first magnification;
[0041] Figure 8 This is a SEM image of the positive electrode material C17 of comparative example 7 of the present invention at the second magnification. DETAILED DESCRIPTION
[0042] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0043] According to a first aspect of the present invention, a positive electrode material is provided, comprising a positive electrode active substance and a coating layer coated on the surface of the positive electrode active substance, wherein the coating layer material is a glass-like phase material and the coating layer material contains phosphorus; the specific surface area reduction rate of the positive electrode active substance after being coated by the coating layer is ≥5%.
[0044] The present invention does not limit the preparation method of the positive electrode material, as long as the surface of the positive electrode active material is coated with a coating layer. For example, the positive electrode material can be obtained by mixing the positive electrode active material and the glass-like phase material and then calcining them.
[0045] The glass-like phase material in the present invention refers to a material having high-temperature melting characteristics. The glass-like phase material can melt at high temperatures and is in a liquid state. The glass-like phase material can be in a glassy state or not after cooling, and the present invention does not make any limitation here, as long as the glass-like phase material can melt at high temperatures.
[0046] It should be noted that glass is an amorphous structure, that is, after being melted at high temperature and cooled to room temperature, the material does not produce crystallization and remains an amorphous structure. However, in the present invention, most components can be melted at high temperatures, and crystallization will occur after cooling, especially when more transition metals are added. Therefore, the glass-like phase material in the present invention cannot be accurately called glass. However, glass crystallization is mostly tiny nanocrystals, and is embedded in the glass matrix, and is still extremely uniform.
[0047] Among them, the specific surface area reduction rate of the positive electrode active material after being coated by the coating layer is ≥5%, that is, when the specific surface area of the positive electrode active material is BET 1 , the specific surface area of the positive electrode material is BET 2 , can satisfy (BET 1 -BET 2 ) / BET 1≥5.0%, and the BET after coating is reduced by at least 5% compared with that before coating.
[0048] In the prior art, the coating material is mostly in the form of particles, with many and small particles, and is coated in an island shape on the outer surface of the positive electrode active material. The material in the coating layer is in the form of particles, with many and small particles, and the specific surface area of the coated positive electrode material is much larger than that of the uncoated positive electrode material. However, the positive electrode material of the present invention has a BET reduction rate of ≥5% after coating compared to before coating, indicating that the coating layer formed by the glass-like phase material is uniform and dense.
[0049] P 2 O 5 Can be used as a network generator for glass-like materials. Compared with B 2 O 3 The formed glass-like phase material and the positive electrode material of the present invention have strong stability under high voltage, especially when the positive electrode material is used in a battery, the normal temperature and high temperature cycle performance of the battery can be significantly improved.
[0050] According to the research of the present invention, the positive electrode material has excellent cycle stability and storage performance at high voltage, and the application of the positive electrode material in the battery is conducive to improving the electrochemical performance of the battery. This is because, on the one hand, the glass-like phase material of the present invention can be melted at high temperature, so that the glass-like phase material is in a liquid state at high temperature and has excellent fluidity and uniformity. When the specific surface area reduction rate of the positive electrode active material after being coated by the coating layer is ≥5%, it means that the glass-like phase material can be evenly spread on the surface of the positive electrode active material, completely cover the surface of the positive electrode active material, and form a uniform and complete coating layer, so that the contact between the electrolyte and the positive electrode active material can be fully isolated, the decomposition of the electrolyte under high voltage and the occurrence of surface side reactions can be reduced, and the dissolution of surface ions can be reduced, thereby effectively improving the structural stability of the positive electrode material, and the cycle stability and storage performance of the positive electrode material under high voltage; on the other hand, the glass-like phase material of the present invention can be melted at high temperature, in a liquid state, and has a certain degree of viscosity, and can be firmly coated on the surface of the positive electrode active material, reducing the shedding and loss of the coating layer during charging and discharging, avoiding the coating layer from losing contact with the positive electrode active material, and further improving the cycle stability of the positive electrode material under high voltage. Therefore, applying the above-mentioned positive electrode material to the battery is conducive to improving the cycle performance, capacity retention rate and safety performance of the battery.
[0051] The present invention does not limit the softening point or melting point of the glass-like phase material, as long as the glass-like phase material can be melted at high temperature. In some embodiments, the softening point of the glass-like phase material is ≤1000°C. This ensures that the melting of the glass-like phase material can be achieved at a temperature not higher than 1000°C, and a coating layer is formed on the surface of the positive active material. The softening temperature of the glass-like phase material is close to the synthesis temperature of the positive active material (for example, the synthesis temperature of lithium nickel manganese oxide is usually ≤1000°C), which can be matched with the preparation temperature of the positive active material to avoid the negative impact of high temperature on the positive active material.
[0052] The present invention does not limit the specific type of the positive electrode active material, and it can be a conventional positive electrode active material in the art. For example, in some embodiments, the positive electrode active material is lithium nickel manganese oxide. Lithium nickel manganese oxide has higher energy density and extremely high cost performance.
[0053] In some embodiments, the voltage window of the positive electrode material is 3.5 to 4.95 V. The positive electrode material has a wide electrochemical window and is particularly suitable for battery systems with high operating voltages. The positive electrode material exhibits good cycle stability and storage performance, which is beneficial to improving the electrochemical performance of the battery.
[0054] The present invention does not limit the specific type of glass-like phase material, as long as it can form a glass-like phase material. Currently, silicon, boron, and phosphorus can form glass alone to form a glass grid skeleton, and other elements can also be filled in the grid skeleton. In some embodiments, the glass-like phase material includes the following components by weight percentage: phosphorus pentoxide (P 2 O 5 ) 40-90%, oxides containing element A 10-60%, alkali metal oxides 0-10%; wherein element A includes at least one of Si, Ce, Be, Te, Ta, Al, Cu, Nb, V, W, Sr, Mg, Ti, La, Ca, Zn, Sb, Se, I, preferably at least one of Ti, V, Cu, Nb, Mo, Ta, W, Te, P, F. At this time, P 2 O 5 As a network generator of glass-like materials (i.e., a continuous network or skeleton), a network system is formed; most of the oxides containing element A serve as network intermediates of glass-like materials (i.e., filled into the skeleton), and a small part can also serve as network generators of glass-like materials, and improve the stability of the coating layer, so that the coating layer remains stable under high voltage; alkali metal oxides mainly serve as network exogenous bodies (i.e., promote the formation of glass-like materials), play the role of providing free oxygen and breaking bonds, and promote the common melting of each component.
[0055] In the prior art, glass mainly includes silicate glass, borate glass and phosphate glass. Among them, the melting temperature of silicate glass is relatively high (>1200℃), which is far higher than the synthesis temperature of lithium nickel manganese oxide (≤1000℃). Borate glass has a low melting temperature. 2 O 3 The softening temperature of the low-temperature sealing glass with boron as the main component is only about 400°C. Although it can be well melted at low temperature and achieve uniform and comprehensive coating of the positive electrode material, the high-voltage stability of the boron element is poor. When used in a high-voltage lithium nickel manganese oxide system, it will produce high-voltage decomposition and even deteriorate the electrochemical performance. It is not suitable for use in a high-voltage lithium nickel manganese oxide system. Phosphate glass has a more suitable softening point (<800-1000°C). The glass-like phase material of the present invention can be considered as a material of phosphate glass combined with multiple elements. It can form a firm, uniform and stable coating layer at ≤1000°C, which is beneficial to improve the cycle stability and storage performance of the positive electrode material under high voltage, and is particularly suitable for high-voltage lithium nickel manganese oxide systems.
[0056] In addition, the glass-like material of the present invention contains P elements, PO 4 3- And element A can effectively improve the electrochemical properties of the positive electrode active material (especially lithium nickel manganese oxide); alkali metals can further enhance the lithium ion conductivity of the glass-like phase material, thereby enhancing the lithium ion conductivity of the coating layer, so that even if the positive electrode active material is wrapped by a dense coating layer, it will not affect the passage of lithium ions too much.
[0057] The present invention does not limit the specific type of the oxide containing element A, as long as it contains element A. For example, in some embodiments, the oxide containing element A includes Be 2 O 3 , MgO, CaO, SrO, TiO 2 、V 2 O 5 CrO 3 、Co 3 O 4 、NiO、CuO、ZnO、ZrO 2 , Nb 2 O 5 、MoO 3 , WO 3 、 2 O 5 ,La 2 O 3 、CeO 2 、Nd 2 O 3 、Al 2 O 3 SnO 2、SiO 2 , Sb 2 O 5 、TeO 2 , SeO 2 ,I 2 O 5 At least one of, preferably TeO 2 、 2 O 5 、Al 2 O 3 , CuO, Nb 2 O 5 、V 2 O 5 , WO 3 、CeO、MgO、TiO 2 At least one of .
[0058] The present invention does not limit the specific type of alkali metal oxide. For example, in some embodiments, the alkali metal oxide includes Li 2 O、Na 2 O.K 2 O, preferably Na 2 O. Li 2 At least one of O.
[0059] The present invention does not impose too many restrictions on the mass content of the coating layer. For example, in some embodiments, the mass of the coating layer is 0.1 to 10 wt %, preferably 0.5 to 5 wt %, of the mass of the positive electrode active material.
[0060] The present invention does not limit the chemical formula of the positive electrode active material, which may be a conventional nickel manganese oxide system in the art. For example, in some embodiments, the chemical formula of the positive electrode active material is Li 1+x Ni 0.5+y Mn 1.5+z M u O w , wherein, -0.1≤x≤0.3, -0.2≤y≤0.2, -0.2≤z≤0.2, 0≤u≤0.2, 3.8≤w≤4.3; wherein M includes at least one of Mg, Al, Ca, Sc, Ti, V, Cr, Fe, Co, Cu, Zn, Ga, Sr, Y, Zr, Nb, Mo, Ru, Ta, W, B, Si, Ge, Sb, Te, P, S, and F, and is preferably at least one of Ti, V, Cu, Nb, Mo, Ta, W, Te, P, and F.
[0061] The present invention does not limit the particle type and size of the positive electrode material, which can be a polycrystalline material and / or a single crystal material. For example, in some embodiments, the positive electrode active material is a single crystal material, and the particle size of the single crystal material is 0.5 to 30 μm, preferably 1 to 10 μm; or, the positive electrode active material is a polycrystalline material, and the particle size of the polycrystalline material is 0.1 to 20 μm, preferably 1 to 10 μm.
[0062] A second aspect of the present invention provides a method for preparing the positive electrode material according to the first aspect, comprising the following steps:
[0063] The positive electrode active material is mixed with the glass-like phase material, and after a first sintering treatment and an annealing treatment, a positive electrode material is obtained; wherein the temperature of the first sintering treatment is 700-1000°C, preferably 800-950°C, and the time is 1-30h, preferably 10-20h; the temperature of the annealing treatment is 400-800°C, preferably 500-600°C, and the time is 1-20h, preferably 5-10h.
[0064] The present invention does not limit the preparation process of the glass-like phase material, and conventional melting methods in the art can be used. For example, in some embodiments, the glass-like phase material is prepared by a method including the following processes: P compound, compound containing element A, and alkali metal compound are uniformly mixed according to a mass ratio to obtain a mixture; the mixture is melted and crushed to obtain a glass-like phase material; wherein the melting treatment temperature is 800-1300°C, and the time is 3-10 hours.
[0065] After the melting process, the material needs to be cooled, and then crushed and sieved to obtain a glass-like material.
[0066] Among them, P compounds refer to compounds other than P 2 O 5 In addition, it also includes compounds that can decompose and eventually form phosphorus pentoxide when sintered at high temperature in air or an oxidizing atmosphere, such as phosphoric acid, monoammonium hydrogen phosphate, diammonium hydrogen phosphate, diammonium hydrogen phosphate, etc., not just the specific compound of phosphorus pentoxide.
[0067] The compound containing element A may be an oxide containing element A, or may be other compounds containing element A, for example, oxides containing element A include Be 2 O 3 , MgO, CaO, SrO, TiO 2 、V 2 O 5 CrO 3 、Co 3 O 4 、NiO、CuO、ZnO、ZrO 2 , Nb2 O 5 、MoO 3 , WO 3 、 2 O 5 ,La 2 O 3 、CeO 2 、Nd 2 O 3 、Al 2 O 3 、SnO2、SiO 2 , Sb 2 O 5 、TeO 2 , SeO 2 ,I 2 O 5 At least one of the above. The compound containing element A also includes a compound containing element A that can be decomposed and oxidized to form an oxide containing element A by high-temperature sintering in an oxygen or air atmosphere. For example, CuO can be obtained from copper acetate, copper sulfate, copper nitrate, copper chloride, copper carbonate, copper phosphate, copper oxalate, etc., not just CuO.
[0068] In addition to alkali metal oxides, alkali metal compounds also include compounds that can decompose and eventually form alkali metal oxides by high-temperature sintering in air or an oxidizing atmosphere, not just the specific oxides. 2 O can be formed from lithium carbonate, lithium hydroxide, lithium oxalate, lithium acetate, lithium citrate, lithium fluoride, etc. at high temperature.
[0069] The present invention does not limit the preparation process of the positive electrode active material, and a conventional sintering method in the art can be used. For example, in some embodiments, a precursor, a lithium source and an additive are added to a high-speed mixer and mixed and stirred until uniform; the mixture is sintered, and after natural cooling, it is crushed and sieved to obtain the positive electrode active material.
[0070] According to a third aspect of the present invention, a positive electrode sheet is provided. The positive electrode sheet comprises the positive electrode material according to the first aspect or the positive electrode material prepared by the preparation method according to the second aspect.
[0071] The positive electrode sheet of the present invention can also be prepared by conventional technical means in the art. Specifically, the above-mentioned positive electrode material, conductive agent, and binder can be uniformly dispersed in a solvent to obtain a positive electrode active layer slurry, and then the positive electrode active layer slurry is coated on at least one functional surface of the positive electrode collector. After drying, the positive electrode sheet of the present invention can be obtained.
[0072] The present invention does not particularly limit the specific types of the conductive agent and the adhesive. The conductive agent, the adhesive and other components can be selected from conventional materials in the field. For example, the conductive agent can be selected from one or more of conductive carbon black, carbon nanotubes, conductive graphite, and graphene, and the adhesive can be selected from one or more of polyvinylidene fluoride (PVDF), acrylic modified PVDF, polyacrylate polymers, polyimide, styrene-butadiene rubber, and styrene-propylene rubber.
[0073] The present invention does not specifically limit the coating method, and any coating method such as gravure coating, extrusion coating, spraying, screen printing, etc. can be used to coat the positive electrode active layer slurry.
[0074] In a fourth aspect, the present invention provides a lithium ion battery, the lithium ion battery comprising the positive electrode sheet provided in the third aspect. In addition to the positive electrode sheet, the lithium ion battery of the present invention also comprises a diaphragm, a negative electrode sheet and an electrolyte. Among them, the composition of the negative electrode sheet can refer to the conventional negative electrode sheet in the art, and the diaphragm can also adopt the diaphragm conventionally used in the art, such as PP film, PE film, etc.
[0075] The lithium-ion battery of the present invention can be prepared by conventional methods in the art. Specifically, the positive electrode sheet, the separator and the negative electrode sheet can be stacked in sequence, and then a battery cell can be obtained through a stacking or winding process, and then the above-mentioned lithium-ion battery can be obtained through baking, liquid injection, formation, packaging and other processes.
[0076] The present invention will be further described below by means of specific examples and comparative examples.
[0077] Example 1
[0078] (1) 10 kg of precursor Ni 0.5 Mn 1.5 (OH) 4 , 2.1kg lithium carbonate and 100g Ta 2 O 5 Add to a high-speed mixer, mix and stir until uniform to obtain a mixture; sinter the mixture at 950°C for 10 hours, and crush and sieve after natural cooling to obtain LiNi 0.5 Mn 1.5 Ta 0.0083 O 4 (positive electrode active material), denoted as A1;
[0079] (2) According to the mass ratio of each component in the target product (glass-like phase material) P 2 O 5 :Li 2 O:SiO 2 :Al 2 O 3 :TiO 2=51:6:12:16.5:14.5 ratio will include diammonium phosphate, lithium carbonate, SiO 2 、Al 2 O 3 、TiO 2 The raw materials including are mixed evenly, melted at 1000℃ for 5h, crushed and sieved after cooling to obtain a glass-like phase material, which is recorded as B1;
[0080] (3) 10 kg of A1 and 100 g of B1 were mixed evenly using a high-speed mixer, sintered at 800 °C for 10 h, cooled to 500 °C at a rate of 3 °C / min and kept at this temperature for 5 h, naturally cooled to room temperature, crushed and sieved to obtain a positive electrode material, recorded as C1.
[0081] Example 2
[0082] The preparation process is basically the same as that of Example 1, except that in step (2), the mass ratio of each component in the target product (glass-like phase material) is P 2 O 5 :Li 2 O:Ta 2 O 5 :Al 2 O 3 =50:7:16:27 ratio will include diammonium phosphate, lithium carbonate, Ta 2 O 5 、Al 2 O 3 The raw materials including are mixed evenly, and other conditions remain unchanged to obtain a glass-like phase material, which is recorded as B2; step (3) 10kg A1 and 100g B2 are mixed evenly using a high-speed mixer, sintered at 930°C for 10h, cooled to 500°C at a rate of 3°C / min and kept warm for 5h, naturally cooled to room temperature, crushed and sieved to obtain a positive electrode material, which is recorded as C2.
[0083] Example 3
[0084] The preparation process is basically the same as that of Example 1, except that in step (2), the mass ratio of each component in the target product (glass-like phase material) is P 2 O 5 :Li 2 O:SiO 2 :Ta 2 O 5 :V 2 O 5 :TeO 2 =45:5:20:5:15:10 ratio will include diammonium phosphate, lithium carbonate, SiO 2 、 2 O 5 、V2 O 5 、TeO 2 The raw materials including are mixed evenly, and other conditions remain unchanged to obtain a glass-like phase material, which is recorded as B3; step (3) 10kg A1 and 100g B3 are mixed evenly using a high-speed mixer, and after sintering at 880°C for 10h, the temperature is reduced to 500°C at a rate of 3°C / min and kept warm for 5h, and other conditions remain unchanged to obtain a positive electrode material, which is recorded as C3.
[0085] Example 4
[0086] The preparation process is basically the same as that of Example 1, except that in step (2), the mass ratio of each component in the target product (glass-like phase material) is P 2 O 5 :Na 2 O:Al 2 O 3 =70:10:20 ratio will include diammonium phosphate, sodium carbonate, Al 2 O 3 The raw materials including are mixed evenly, and other conditions remain unchanged to obtain a glass-like phase material, which is recorded as B4; step (3) uses a high-speed mixer to mix 10kgA1 and 100g B4 materials evenly, sinter at 850°C for 10h, and then naturally cool to room temperature and then crush and sieve to obtain a positive electrode material, which is recorded as C4.
[0087] Example 5
[0088] The preparation process is basically the same as that of Example 1, except that in step (2), the mass ratio of each component in the target product (glass-like phase material) is P 2 O 5 :Li 2 O:SiO 2 :Nb 2 O 5 :MgO:La 2 O 3 =45:8:19:8:10:10 ratio will include diammonium phosphate, lithium carbonate, SiO 2 , Nb 2 O 5 、MgO、La 2 O 3 The raw materials including are mixed evenly, and other conditions remain unchanged to obtain a glass-like phase material, which is recorded as B5; in step (3), 10 kg of A1 and 100 g of B5 are mixed evenly using a high-speed mixer, sintered at 870 ° C for 10 h, cooled to 400 ° C at a rate of 3 ° C / min and kept warm for 5 h, naturally cooled to room temperature, and then crushed and sieved to obtain a positive electrode material, which is recorded as C5.
[0089] Example 6
[0090] The preparation process is basically the same as that of Example 1, except that in step (3), 10 kg of A1 and 10 g of B1 are mixed evenly using a high-speed mixer, sintered at 860 ° C for 6 h, cooled to 500 ° C at a rate of 3 ° C / min and kept warm for 5 h, naturally cooled to room temperature, crushed and sieved to obtain a positive electrode material, recorded as C6.
[0091] Example 7
[0092] The preparation process is basically the same as that of Example 1, except that in step (3), 5 kg of A1 and 100 g of B1 are evenly mixed using a high-speed mixer, sintered at 900 °C for 10 h, cooled to 500 °C at a rate of 3 °C / min and kept warm for 5 h, naturally cooled to room temperature, crushed and sieved to obtain a positive electrode material, recorded as C7.
[0093] Example 8
[0094] The preparation process is basically the same as that of Example 1, except that in step (3), 2 kg of A1 and 100 g of B1 are mixed evenly using a high-speed mixer, sintered at 900 °C for 10 h, cooled to 500 °C at a rate of 3 °C / min and kept warm for 5 h, naturally cooled to room temperature, crushed and sieved to obtain a positive electrode material, recorded as C8.
[0095] Example 9
[0096] The preparation process is basically the same as that of Example 1, except that in step (3), 1 kg of A1 and 100 g of B1 are evenly mixed using a high-speed mixer, sintered at 900 °C for 10 h, cooled to 500 °C at a rate of 3 °C / min and kept warm for 5 h, naturally cooled to room temperature, crushed and sieved to obtain a positive electrode material, recorded as C9.
[0097] Example 10
[0098] (1) 10 kg of precursor Ni 0.5 Mn 1.5 (OH) 4 , 2.25kg lithium carbonate and 300g NH 4 H 2 PO 4 Add to high-speed mixer, mix and stir until uniform, sinter the mixture at 950℃ for 10h, and crush and sieve after natural cooling to obtain LiNi 0.5 Mn 1.5 P 0.0139 O 4 (positive electrode active material), denoted as A2;
[0099] (2) According to the mass ratio P of each component in the target product (glass-like material) 2 O 5:Li 2 O:SiO 2 :Al 2 O 3 :TiO 2 =51:6:12:16.5:14.5 ratio will include diammonium phosphate, lithium carbonate, SiO 2 、Al 2 O 3 、TiO 2 The raw materials including are mixed evenly, melted at 1000℃ for 5h, crushed and sieved after cooling to obtain a glass-like phase material, which is recorded as B1;
[0100] (3) Use a high-speed mixer to mix 10 kg of A2 and 100 g of B1 evenly, sinter at 900 °C for 10 h, cool to 500 °C at a rate of 3 °C / min and keep warm for 5 h. After naturally cooling to room temperature, crush and sieve to obtain a positive electrode material, which is recorded as C10.
[0101] Embodiment 11
[0102] The preparation process is basically the same as that of Example 10, except that in step (2), the mass ratio of each component in the target product (glass-like phase material) is P 2 O 5 :Li 2 O:SiO 2 :Ta 2 O 5 :V 2 O 5 :TeO 2 =45:5:20:5:15:10 ratio will include diammonium phosphate, lithium carbonate, SiO 2 、 2 O 5 、V 2 O 5 、TeO 2 The raw materials including are mixed evenly, and other conditions remain unchanged to obtain a glass-like phase material, which is recorded as B3; step (3) using a high-speed mixer to mix 5kg A2 and 100g B3 evenly, sintering at 880°C for 10h, cooling to 500°C at a rate of 3°C / min and keeping warm for 5h, naturally cooling to room temperature, and then crushing and sieving to obtain a positive electrode material, which is recorded as C11.
[0103] Example 12
[0104] The preparation process is basically the same as that of Example 10, except that in step (2), the mass ratio of each component in the target product (glass-like phase material) is P 2 O 5 :Li 2 O:SiO 2:Nb 2 O 5 :MgO:La 2 O 3 =45:8:19:8:10:10 ratio will include diammonium phosphate, lithium carbonate, SiO 2 :Nb 2 O 5 :MgO:La 2 O 3 The raw materials including are mixed evenly, and other conditions remain unchanged to obtain a glass-like phase material, which is recorded as B5; in step (3), 2kg A2 and 100g B5 materials are mixed evenly using a high-speed mixer, sintered at 970°C for 10h, cooled to 500°C at a rate of 3°C / min and kept warm for 5h, naturally cooled to room temperature, and then crushed and sieved to obtain a positive electrode material, which is recorded as C12.
[0105] Embodiment 13
[0106] The preparation process is basically the same as that of Example 1, except that in step (1), 10 kg of precursor Ni 0.5 Mn 1.5 (OH) 4 , 2.25kg lithium carbonate and 43g Nb 2 O 5 , 220g NH 4 H 2 PO 4 Add to high-speed mixer, mix and stir until uniform, sinter the mixture at 950℃ for 10h, and crush and sieve after natural cooling to obtain LiNi 0.5 Mn 1.5 Nb 0.0059 P 0.0138 O 4 (positive electrode active material), denoted as A3; step (3) using a high-speed mixer to evenly mix 5kg A3 and 100g B1 material, sintering at 900°C for 10h, cooling to 500°C at a rate of 3°C / min and keeping warm for 5h, naturally cooling to room temperature, and then crushing and sieving to obtain a positive electrode material, denoted as C13.
[0107] Embodiment 14
[0108] The preparation process is basically the same as that of Example 1, except that in step (1), 10 kg of precursor Ni 0.5 Mn 1.5 (OH) 4 , 2.25kg lithium carbonate and 86g MoO 3 Add to a high-speed mixer, mix and stir until uniform, sinter the mixture at 900°C for 10 hours, and crush and sieve after natural cooling to obtain LiNi 0.5 Mn1.5 Mo 0.0055 P 0.0138 O 4 (positive electrode active material), denoted as A4; step (3) using a high-speed mixer to mix 5kg A4 and 100g B1 material evenly, sintering at 870°C for 10h, cooling to 500°C at a rate of 3°C / min and keeping warm for 5h, naturally cooling to room temperature, and then crushing and sieving to obtain a positive electrode material, denoted as C14.
[0109] Comparative Example 1
[0110] 10 kg of precursor Ni 0.5 Mn 1.5 (OH) 4 , 2.1kg lithium carbonate and 100g Ta 2 O 5 The mixture was added into a high-speed mixer and mixed and stirred until uniform to obtain a mixture; the mixture was sintered at 950°C for 10 hours, and after natural cooling, it was crushed and sieved to obtain Ta-doped modified lithium nickel manganese oxide positive electrode material LiNi 0.5 Mn 1.5 Ta 0.0083 O 4 , denoted as A1.
[0111] Comparative Example 2
[0112] 10 kg of precursor Ni 0.5 Mn 1.5 (OH) 4 , 2.25kg lithium carbonate and 300g NH 4 H 2 PO 4 Add to high-speed mixer, mix and stir until uniform, sinter the mixture at 950℃ for 10h, and crush and sieve after natural cooling to obtain LiNi 0.5 Mn 1.5 P 0.0139 O 4 , denoted as A2.
[0113] Comparative Example 3
[0114] 10 kg of precursor Ni 0.5 Mn 1.5 (OH) 4 , 2.25kg lithium carbonate and 43g Nb 2 O 5 , 220g NH 4 H 2 PO 4 Add to high-speed mixer, mix and stir until uniform, sinter the mixture at 950℃ for 10h, and crush and sieve after natural cooling to obtain LiNi0.5 Mn 1.5 Nb 0.0059 P 0.0138 O 4 , denoted as A3.
[0115] Comparative Example 4
[0116] 10 kg of precursor Ni 0.5 Mn 1.5 (OH) 4 , 2.25kg lithium carbonate and 86g MoO 3 , add to a high-speed mixer, mix and stir until uniform. Sinter the mixture at 900°C for 10 hours, cool naturally, crush and sieve to obtain LiNi 0.5 Mn 1.5 Mo 0.0108 P 0.0138 O 4 , recorded as A4.
[0117] Comparative Example 5
[0118] Use a high speed mixer to mix 10kg A1 with 100g P 2 O 5 The mixture was mixed evenly, sintered at 900°C for 10 h, cooled to 500°C at a rate of 3°C / min and kept at this temperature for 5 h. After naturally cooling to room temperature, the mixture was crushed and sieved to obtain the positive electrode material, which was recorded as C15.
[0119] Comparative Example 6
[0120] 5kg A1 and 100g TiO 2 The mixture was mixed evenly, sintered at 900°C for 10 h, cooled to 500°C at a rate of 3°C / min and kept at this temperature for 5 h. After naturally cooling to room temperature, the mixture was crushed and sieved to obtain the positive electrode material, which was recorded as C16.
[0121] Comparative Example 7
[0122] 5 kg of A1 and a mixture of By (51 g P 2 O 5 , 6g Li 2 O, 12g SiO 2 、16.5g Al 2 O 3 , 14.5g TiO 2 ) were mixed evenly, sintered at 500°C for 10 h, naturally cooled to room temperature, crushed and sieved to obtain a positive electrode material, which was recorded as C17.
[0123] Comparative Example 8
[0124] (1) According to the mass ratio of each component in the target product (glass-like material) 2 O 3 :Li 2 O:SiO 2 :Al 2 O 3 :TiO 2 =51:6:12:16.5:14.5 ratio will include B 2 O 3 , lithium carbonate, SiO 2 、Al 2 O 3 、TiO 2 The raw materials including are mixed evenly, melted at 1000°C for 5h, crushed and sieved after cooling to obtain a glass-like phase material, which is recorded as Bx.
[0125] (2) 10 kg of A1 and 100 g of Bx were mixed evenly using a high-speed mixer, sintered at 900 °C for 10 h, cooled to 500 °C at a rate of 3 °C / min and kept at this temperature for 5 h, naturally cooled to room temperature, crushed and sieved to obtain a positive electrode material, recorded as C18.
[0126] Test example
[0127] 1. BET
[0128] The specific surface area (BET) was measured by nitrogen adsorption and desorption of the material using TristarⅡ-3020. The specific surface area of the positive electrode active material before coating is BET 1 The specific surface area of the coated positive electrode active material (i.e. positive electrode material) is BET 2 , according to σ(%)=(BET 1 -BET 2 ) / BET 1 Calculate σ.
[0129] 2. Electrochemical performance test: The charge and discharge capacity, first efficiency and cycle retention rate of the present invention were tested using a Wuhan Blue Electric charge and discharge instrument, 3.5-4.95V, and a nominal capacity of 145mAh / g.
[0130] 3. 28-day storage gas production test: After the soft-pack battery is fully formed, the air bag is removed and sealed, and the volume and initial capacity after formation are tested. Charge to 4.95V, and test the volume of the soft-pack battery after 28 days of storage. The ratio of the volume change before and after storage to the initial capacity is the 28-day storage gas production.
[0131] 4. 28-day storage capacity retention rate: After the soft-pack full battery is formed, the air bag is removed and sealed, and the initial capacity after formation is tested. Charge to 4.95V, and test the remaining capacity of the battery after 28 days of storage. The ratio of the remaining battery capacity to the initial capacity is the 28-day storage capacity retention rate.
[0132] The test results are shown in Table 1
[0133] Table 1
[0134]
[0135] SEM photos of A1 are shown in Figure 1 and Figure 2 , which is a uniform octahedral structure, and the BET of A1 is 0.5244m 2 / g; SEM photo of the positive electrode material C1 of Example 1 is shown in Figure 3 and Figure 4 As can be seen from the figure, after coating, the morphology of the nickel positive electrode active material particles has changed slightly, especially the surface of some positive electrode active material particles has formed planes and bulges with non-regular octahedral characteristics, proving that the glass-like phase material has formed a good coating on the surface of the positive electrode active material. The fine particles on the surface of the positive electrode active material particles are mainly caused by the crushing process, not the raw material particles of the coating; in the specific production process, the fine crushed objects on the surface can be removed by airflow powder selection.
[0136] The SEM photo of the positive electrode material C7 of Example 7 is shown in Figure 5 and Figure 6 ; The SEM photo of the positive electrode material C17 of Comparative Example 7 is shown in Figure 7 and Figure 8 As can be seen from the figure, there are a large number of granular substances on the surface of the positive electrode active material, and the coating materials do not produce a melting effect and do not form a dense coating on the positive electrode active material.
[0137] According to Table 1, we can see that:
[0138] 1. By comparing the embodiments and comparative examples, it can be seen that since comparative examples 1-4 do not contain a coating layer, the electrochemical performance of the positive electrode material in the full battery, especially the 2C cycle retention rate (100 cycles), the number of cycles when the capacity retention rate is 80% under 1C conditions, and the 28-day storage capacity retention rate are poor, the gas production in 28 days increases, and the safety is poor; Examples 1-14 are beneficial to improving the electrochemical performance and safety performance of the battery by setting a coating layer.
[0139] 2. By comparing Examples 1-14, it can be seen that controlling the ratio of the glass-like phase material to the positive electrode active material is beneficial to taking into account both the electrochemical performance of the positive electrode material in the half-cell and the electrochemical performance in the full cell.
[0140] 3. By comparing Examples 1-14 and Comparative Examples 5-6, it can be seen that when a single component of phosphorus pentoxide or titanium oxide is used as the coating material, it is difficult to achieve σ(%) ≥ 5.0%, which is not conducive to the electrochemical performance. The inventors believe that due to the poor stability of the single component, part of the phosphorus pentoxide or titanium oxide is doped into the positive electrode active material, making it difficult to form a complete coating on the surface of the positive electrode active material.
[0141] 4. By comparing Examples 1-14 and Comparative Example 7, it can be seen that since Comparative Example 7 is sintered at 500° C., it is difficult to form a glass-like phase and difficult to form a uniform and complete coating on the surface of the positive electrode active material.
[0142] 5. By comparing Examples 1-14 and Comparative Example 8, it can be seen that compared with the prior art using boron compounds as coating layer materials, applying the positive electrode material of this embodiment to the battery can further improve the electrochemical performance of the positive electrode material in the full battery.
[0143] The preferred specific embodiments and experimental verification of the present invention are described in detail above. It should be understood that ordinary technicians in this field can make many modifications and changes based on the concept of the present invention without creative work. Therefore, all technical solutions that can be obtained by technicians in this technical field based on the concept of the present invention through logical analysis, reasoning or limited experiments on the basis of the prior art should be within the scope of protection determined by the claims.
Claims
1. A positive electrode material, characterized in that: The invention comprises a positive electrode active material and a coating layer coated on the surface of the positive electrode active material, wherein the coating layer material is a glass-like phase material and the coating layer material contains phosphorus; the mass of the coating layer is 0.5 to 5 wt% of the mass of the positive electrode active material; The specific surface area reduction rate of the positive electrode active material after being coated by the coating layer is ≥5%; The glass-like phase material comprises the following components by weight percentage: Phosphorus pentoxide 40-90%, oxides containing element A 10-60%, alkali metal oxides 0-10%; Wherein, the oxide containing element A includes at least one of Be2O3, MgO, CaO, SrO, TiO2, V2O5, CrO3, Co3O4, NiO, ZrO2, Nb2O5, Ta2O5, La2O3, CeO2, Nd2O3, Al2O3, SiO2, Sb2O5, TeO2, SeO2, and I2O5; The alkali metal oxide includes at least one of Li2O, Na2O, and K2O; The voltage window of the positive electrode material is 3.5 to 4.95V; The positive electrode material is prepared by a method comprising the following steps: The glass-like phase material is obtained by melting and crushing a mixture of a P compound, a compound containing an A element and an alkali metal compound in sequence; wherein the temperature of the melting treatment is 800-1300°C and the time is 3-10 hours; the glass-like phase material is mixed with a positive electrode active material, and after a first sintering treatment and an annealing treatment, the positive electrode material is obtained; wherein the temperature of the first sintering treatment is 700-1000°C and the time is 1-30 hours; the temperature of the annealing treatment is 400-800°C and the time is 1-20 hours.
2. The positive electrode material according to claim 1, characterized in that The softening point of the glass-like phase material is ≤1000°C.
3. The positive electrode material according to claim 1, characterized in that The chemical formula of the positive electrode active material is Li 1+ x Ni 0.5+y Mn 1.5+z M u O w , where -0.1≤x≤0.3, -0.2≤y≤0.2, -0.2≤z≤0.2, 0≤u≤0.2, 3.8≤w≤4.3; Among them, M includes at least one of Mg, Al, Ca, Sc, Ti, V, Cr, Fe, Co, Cu, Zn, Ga, Sr, Y, Zr, Nb, Mo, Ru, Ta, W, B, Si, Ge, Sb, Te, P, S, and F.
4. The positive electrode material according to claim 2, characterized in that The positive electrode active material is a single crystal material, and the particle size of the single crystal material is 0.5 to 30 μm; or The positive electrode active material is a polycrystalline material, and the particle size of the polycrystalline material is 0.1 to 20 μm.
5. A method for preparing the positive electrode material according to any one of claims 1 to 4, characterized in that: The following steps are involved: 1) mixing the P compound, the compound containing the A element, and the alkali metal compound uniformly according to a mass ratio to obtain a mixture; melting and crushing the mixture to obtain the glass-like phase material; wherein the melting temperature is 800 to 1300° C. and the time is 3 to 10 hours 2) The positive electrode active material is mixed with the glass-like phase material, and after a first sintering treatment and an annealing treatment, the positive electrode material is obtained; wherein the temperature of the first sintering treatment is 700-1000°C and the time is 1-30 hours; the temperature of the annealing treatment is 400-800°C and the time is 1-20 hours.
6. The preparation method according to claim 5, characterized in that: The P compound is phosphorus pentoxide, or at least one of compounds that can form phosphorus pentoxide after sintering in air or an oxidizing atmosphere; The compound containing element A is an oxide containing element A, or at least one of compounds that can form an oxide containing element A after sintering in air or an oxidizing atmosphere; The alkali metal compound is an alkali metal oxide, or at least one compound that can form an alkali metal oxide after sintering in air or an oxidizing atmosphere.
7. The preparation method according to claim 6, characterized in that: The P compound includes at least one of phosphorus pentoxide, phosphoric acid, ammonium monohydrogen phosphate, ammonium dihydrogen phosphate, and diammonium hydrogen phosphate; The alkali metal compound includes at least one of lithium carbonate, lithium hydroxide, lithium oxalate, lithium acetate, lithium citrate, lithium fluoride and sodium carbonate.
8. A positive electrode sheet, characterized in that: The positive electrode sheet comprises the positive electrode material according to any one of claims 1 to 4 or the positive electrode material prepared by the preparation method according to any one of claims 5 to 7.
9. A lithium ion battery, characterized in that: The lithium-ion battery comprises the positive electrode sheet according to claim 8.