A heat insulation composite material and a preparation method thereof
By introducing hydrophobic aerogel felt and glass fiber reinforced polypropylene composite materials into GMT materials, the problems of large quality, non-recyclable and complex processes of traditional logistics vehicle insulation materials are solved, and high-efficiency thermal insulation and environmental protection are achieved Preparation of thermal insulation composite materials.
Patent Information
- Application Number
- CN202310607931.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-05-26
AI Technical Summary
Traditional logistics vehicle insulation materials are of high quality and are inconvenient for transportation and use, polyurethane materials are not recyclable, and the combination of thermoplastic resin and glass fiber in GMT materials is difficult, resulting in complex preparation process and environmental pollution, limited amount of aerogel layer added and combined Poor strength affects the mechanical properties of the material.
Using glass fiber reinforced polypropylene composite material as the surface layer and the bottom layer, the core layer is GMT aerogel felt, including lightweight GMT material and covered hydrophobic aerogel. Epoxy-containing aerogel is prepared by KH560 surface modification. , combine resin powder to form a composite layer, improve the bonding strength between layers, reduce the use of adhesives, and enhance thermal insulation performance.
The insulation, mechanical properties and environmental protection of the material are improved, and the problems of insufficient addition amount and poor bonding strength of the aerogel layer are solved, thereby achieving efficient thermal insulation and environmental protection technology.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite materials, and in particular relates to a heat insulating composite material and a preparation method thereof. Background Art
[0002] Traditional thermal insulation materials for logistics vehicles use foam boards and composite steel plates. Although they have a certain thermal insulation effect, the thermal insulation composite material is too heavy, which brings inconvenience to transportation and use. Polyurethane is also widely used in the field of thermal insulation materials, but polyurethane cannot be recycled and is not environmentally friendly. In addition, since the thermal insulation materials for logistics vehicles need to meet mechanical properties such as high tear resistance and impact resistance, when using multi-layer materials, there are also high requirements for the bonding strength between different layers, as well as long-distance transportation to achieve good thermal insulation performance. Therefore, there are also high requirements for the thermal insulation material performance of the material.
[0003] GMT material is a new type of composite material composed of glass fiber felt and thermoplastic resin. It has great potential in the application field of thermal insulation materials for logistics vehicles due to its high strength, high impact toughness, good load-bearing capacity, high temperature resistance, light weight, recyclability, not easy to deform, good sound absorption and sound insulation, and no odor. When only glass fiber felt is used, although it can play a certain thermal insulation effect, it has the disadvantages of low thermal insulation efficiency and large heat loss. In addition, it is difficult to combine thermoplastic resin and glass fiber in GMT material. When preparing glass fiber felt, more adhesives need to be used, which will cause environmental pollution and increase the difficulty of the preparation process, such as CN202220041123.X.
[0004] In response to the above problems, some studies have set an aerogel layer when preparing thermal insulation composite materials, such as CN217105608U and CN208867647U. However, this setting has the following problems: (1) Aerogel cannot be added in large quantities, because excessive aerogel addition will require an increase in the amount of binder; (2) Aerogel is set as a single layer and the aerogel content in this layer is relatively high, which will lead to a decrease in the bonding strength between the aerogel insulation layer and the surface layer, and the mechanical properties of the prepared material are poor. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a thermal insulation composite material and a preparation method thereof. The specific technical scheme is as follows:
[0006] A heat insulation composite material, characterized in that it comprises a surface layer, a core layer and a bottom layer, wherein the core layer is arranged between the surface layer and the bottom layer; the surface layer and the bottom layer are both glass fiber reinforced polypropylene composite materials;
[0007] The core layer is a GMT aerogel felt, which includes a lightweight GMT material and an aerogel covering the surface of the lightweight GMT material, and the product after the silica sol is dried is an aerogel;
[0008] The lightweight GMT material comprises a blended fiber felt and a composite layer of aerogel and resin powder, wherein the composite layer comprises two layers arranged on the upper and lower surfaces of the blended fiber felt.
[0009] The mass ratio of aerogel to resin powder in the composite layer is 1:10-20.
[0010] The resin powder in the composite layer is polypropylene resin powder.
[0011] The core layer has a thickness of about 3 to 30 mm, and the surface layer and the bottom layer have a thickness of 0.5 to 2 mm.
[0012] The aerogel in the composite layer is a hydrophobic aerogel. The hydrophobic aerogel is an epoxy-containing aerogel prepared by surface modification of the aerogel with KH560. The preparation method is to soak the aerogel in 5-10wt% KH560 for 2-8h and then dry it at 50-60°C.
[0013] The hydrophobic aerogel contains epoxy groups, which are randomly condensed with alcoholic hydroxyl groups in the silica sol, thereby further enhancing the bonding strength between the composite layer and the aerogel.
[0014] The present invention also provides a method for preparing a heat-insulating composite material, comprising the following steps:
[0015] (1) Preparation of lightweight GMT material: modified polypropylene fiber and glass fiber are blended to prepare a blended fiber felt, a layer of mixed powder of resin powder and aerogel is spread on the surface of the blended fiber felt, and a lightweight GMT material is obtained after impregnation, hot pressing and baking;
[0016] (2) Preparation of GMT aerogel felt: The lightweight GMT material is impregnated and mixed with the silica sol solution, and after the silica sol solution is gelled, the GMT aerogel felt is obtained by drying;
[0017] (3) Preparation of glass fiber reinforced polypropylene composite material: polypropylene resin, carbon black M717 and antioxidant (a mixture of the antioxidant 1010 and the antioxidant 168 in a mass ratio of 1:1) are uniformly mixed and granulated, and then prepared into a resin film, and the resin film, glass fiber mat and resin film are laid in sequence, hot pressed, cooled and shaped to obtain a glass fiber reinforced polypropylene composite material;
[0018] (4) Laying the glass fiber reinforced polypropylene composite material, the GMT aerogel felt and the glass fiber reinforced polypropylene composite material in sequence and compression molding them to obtain the thermal insulation composite material.
[0019] The resin powder added in (1) is polypropylene resin powder, which can fully impregnate the surface of the blended fiber felt with the resin powder. After subsequent heating and hot pressing, the polypropylene resin and aerogel can fully wrap the blended fiber felt.
[0020] The mixed mass ratio of the modified polypropylene fiber and the glass fiber in (1) is 2-6:3-8; the blended felt contains polypropylene fiber, which has viscosity during hot pressing, which can provide a stronger bonding strength with the composite layer on the one hand, and facilitate the control of the thickness of the overall thermal insulation composite material on the other hand;
[0021] The preparation method of the modified polypropylene fiber in (1) is as follows: 90-95 parts of polypropylene resin, 2-6 parts of polybutadiene, 0.1-1 parts of azobisisobutyronitrile, 0.1-1 parts of cyclic acid anhydride type and 0.1-1 parts of bisphenol A type cyanate are mixed, the temperature and pressure are raised to 130-140°C and 15-20MPa, and then the mixture is rapidly stirred to obtain a modified polypropylene resin, and then the modified polypropylene fiber is obtained by spinning. The modification of the polypropylene fiber makes the polypropylene fiber and the glass fiber more evenly mixed.
[0022] The impregnation in (1) can be carried out by electrostatic dry impregnation, which can make the resin powder more uniform on the surface of the fiber felt.
[0023] In the above (2), surface hydrophobic modification can be carried out in the gel stage as required.
[0024] The drying temperature in (2) is 90-120°C.
[0025] The contents of the components in (3) are respectively 97.5 wt% of polypropylene resin, 2 wt% of carbon black M717, and 0.5 wt% of antioxidant.
[0026] Aerogel can also be added to the glass fiber reinforced polypropylene composite material in (3), and the contents of the components are respectively 94.5wt% of polypropylene resin, 2wt% of carbon black M717, 0.5wt% of antioxidant and 3wt% of aerogel.
[0027] The molding temperature in (4) is 180-200° C., the hot pressing pressure is 3-5 MPa, and the hot pressing time is 1-4 min.
[0028] Compared with the prior art, the technical solution in the present invention has the following advantages:
[0029] (1) In the present invention, aerogel dry powder is pre-mixed into the resin powder during the preparation of the core layer, thereby solving the problems in the prior art of poor mechanical properties of the material due to the separate provision of the aerogel layer and insufficient thermal insulation performance due to the inability to add too much aerogel when mixed with other components, thereby making the prepared material have excellent thermal insulation and heat insulation properties.
[0030] (2) The fiber felt of the present invention is a blended felt of polypropylene resin and glass fiber felt. The polypropylene resin is evenly distributed in the fiber felt. The polypropylene resin can also have a bonding effect through hot pressing, so that the interface bonding strength between the core layers is relatively high, and it is also beneficial to control the overall thickness of the composite material through hot pressing.
[0031] (3) The present invention introduces at least two aerogel layers into the GMT material and connects different aerogel layers through chemical bonds, thereby further enhancing the interface bonding strength between different layers. At the same time, the lightweight aerogel component is evenly attached to the surface of the glass fiber felt, further improving the thermal insulation performance of the GMT material.
[0032] (4) The process of the present invention allows the resin powder in the core layer material and the resin in the surface layer material to be bonded to each other through the molten polypropylene resin during hot pressing, which effectively solves the problem of difficult interface bonding of GMT materials, does not require the use of additional adhesives, and is more environmentally friendly.
[0033] (5) The composite material provided by the present invention has high interlayer interface bonding strength, excellent mechanical properties such as impact resistance and tear resistance, and increases the service life of the thermal insulation composite material. DETAILED DESCRIPTION
[0034] The aerogel in the composite layer is a hydrophobic aerogel. The hydrophobic aerogel is an epoxy-containing aerogel prepared by surface modification of the aerogel with KH560. The preparation method is to soak the aerogel in 5wt% KH560 for 4 hours and then dry it at 60°C.
[0035] The present invention will be further described below in conjunction with specific embodiments.
[0036] Example 1
[0037] (1) Preparation of lightweight GMT materials:
[0038] Polypropylene resin, polybutadiene, azobisisobutyronitrile, cyclic anhydride type and bisphenol A type cyanate were mixed in a mass ratio of 92:6:1:0.5:0.5, and then the temperature and pressure were raised to 130°C, and then the mixture was rapidly stirred at 15MPa to obtain modified polypropylene resin, which was then subjected to spinning treatment to obtain modified polypropylene fiber for use; then glass fiber and modified polypropylene fiber were selected in a mass ratio of 1:1 and mixed evenly, and then carded, laid and needled to obtain 3000g / m 2 The blended fiber felt is cut as needed for later use; the mixed powder of hydrophobic aerogel modified by kH560 and polypropylene resin powder is sprayed on the surface of the blended fiber felt at a mass ratio of 1:15 between aerogel and polypropylene resin, and the spraying amount is 100g / m 2, a layer of mixed powder is evenly spread on its surface, and the powder is quickly impregnated into the felt by electrostatic dry impregnation, wherein the impregnation time is 15s and the travel speed is 5m / min. The mixed felt obtained above is reinforced by double-sided needle punching, and the needle punching is 50 punctures / cm up and down. 2 The needle punching depth is 15 mm up and down. The preheated felt plate is heated to 150°C and then hot-pressed for 4 minutes by continuous roller pressing. It is then placed in an oven and heated and baked at 170°C for 60 minutes to obtain a 15 mm thick lightweight GMT material.
[0039] (2) GMT aerogel felt:
[0040] The lightweight GMT material is placed in a suitable container in the form of a roll, and the prepared silica sol solution is injected into the coated lightweight GMT material to exhaust the air in the lightweight GMT material. After the solution is gelled, it is dried by supercritical fluid to obtain the GMT aerogel felt;
[0041] (3) Preparation of glass fiber reinforced polypropylene composite materials:
[0042] Polypropylene resin, carbon black M717, antioxidant (a mixture of the antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1) and aerogel were taken in a mass ratio of 94.5:2:0.5:3, stirred evenly at 500r / min, and melted and extruded to prepare a resin film. The resin film / glass fiber mat / resin film were laid in sequence, the molding equipment was heated to 200°C, the resin film was fully melted, hot pressed at a pressure of 5MPa, cooled and shaped, and a glass fiber mat reinforced polypropylene composite material was obtained;
[0043] (4) Hot pressing compound:
[0044] A layer of glass fiber reinforced polypropylene material composite material, a layer of aerogel reinforced GMT composite material and a glass fiber reinforced polypropylene material composite material are laid in sequence, and are compression molded by a double steel belt continuous press. The compression molding is performed at a hot pressing temperature of 200°C, a hot pressing pressure of 4 MPa and a hot pressing time of 3 minutes. The thermal insulation composite material is obtained through hot pressing composite shaping.
[0045] Example 2
[0046] (1) Preparation of lightweight GMT materials:
[0047] Polypropylene resin, polybutadiene, azobisisobutyronitrile, cyclic anhydride type and bisphenol A type cyanate were mixed in a mass ratio of 92:6:1:0.5:0.5, and then the temperature and pressure were raised to 130°C, and then the mixture was rapidly stirred at 15MPa to obtain modified polypropylene resin, which was then subjected to spinning treatment to obtain modified polypropylene fiber for use; then glass fiber and modified polypropylene fiber were selected in a mass ratio of 1:1 and mixed evenly, and then carded, laid and needled to obtain 3000g / m2 The blended fiber felt is cut as needed for later use; the mixed powder of hydrophobic aerogel modified by kH560 and polypropylene resin powder is sprayed on the surface of the blended fiber felt at a mass ratio of 1:20 between aerogel and polypropylene resin, and the spraying amount is 100g / m 2 , a layer of mixed powder is evenly spread on its surface, and the powder is quickly impregnated into the felt by electrostatic dry impregnation, wherein the impregnation time is 15s and the travel speed is 5m / min. The mixed felt obtained above is reinforced by double-sided needle punching, and the needle punching is 50 punctures / cm up and down. 2 The needle punching depth is 15 mm up and down. The preheated felt plate is heated to 150°C and then hot-pressed for 4 minutes by continuous roller pressing. It is then placed in an oven and heated and baked at 170°C for 60 minutes to obtain a 15 mm thick lightweight GMT material.
[0048] (2) Preparation of GMT aerogel felt:
[0049] The lightweight GMT material is placed in a suitable container in the form of a roll or a flat surface, and the prepared silica sol solution is injected into the laid lightweight GMT material to exhaust the air in the lightweight GMT material. After the solution is gelled, it is dried by supercritical fluid to obtain the GMT aerogel felt;
[0050] (3) Preparation of glass fiber reinforced polypropylene composite materials:
[0051] Polypropylene resin, carbon black M717, antioxidant (a mixture of the antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1) and aerogel were taken in a mass ratio of 94.5:2:0.5:3, stirred evenly at 500r / min, and melted and extruded to prepare a resin film. The resin film / glass fiber mat / resin film were laid in sequence, the molding equipment was heated to 200°C, the resin film was fully melted, hot pressed at a pressure of 5MPa, cooled and shaped, and a glass fiber mat reinforced polypropylene composite material was obtained;
[0052] (4) Hot pressing compound:
[0053] A layer of glass fiber reinforced polypropylene material composite material, a layer of aerogel reinforced GMT composite material and a glass fiber reinforced polypropylene material composite material are laid in sequence, and are compression molded by a double steel belt continuous press. The compression molding is performed at a hot pressing temperature of 200°C, a hot pressing pressure of 4 MPa and a hot pressing time of 3 minutes. The thermal insulation composite material is obtained through hot pressing composite shaping.
[0054] Example 3
[0055] (1) Preparation of lightweight GMT materials:
[0056] Polypropylene resin, polybutadiene, azobisisobutyronitrile, cyclic anhydride type and bisphenol A type cyanate were mixed in a mass ratio of 92:6:1:0.5:0.5, and then the temperature and pressure were raised to 130°C, and then the mixture was rapidly stirred at 15MPa to obtain modified polypropylene resin, which was then subjected to spinning treatment to obtain modified polypropylene fiber for use; then glass fiber and modified polypropylene fiber were selected in a mass ratio of 1:1 and mixed evenly, and then carded, laid and needled to obtain 3000g / m 2 The blended fiber felt is cut as needed for later use; the mixed powder of hydrophobic aerogel modified by kH560 and polypropylene resin powder is sprayed on the surface of the blended fiber felt at a mass ratio of 1:10 between aerogel and polypropylene resin, and the spraying amount is 100g / m 2 , a layer of mixed powder is evenly spread on its surface, and the powder is quickly impregnated into the felt by electrostatic dry impregnation, wherein the impregnation time is 15s and the travel speed is 5m / min. The mixed felt obtained above is reinforced by double-sided needle punching, and the needle punching is 50 punctures / cm up and down. 2 The needle punching depth is 15 mm up and down. The preheated felt plate is heated to 150°C and then hot-pressed for 4 minutes by continuous roller pressing. It is then placed in an oven and heated and baked at 170°C for 60 minutes to obtain a 15 mm thick lightweight GMT material.
[0057] (2) Preparation of GMT aerogel felt:
[0058] The lightweight GMT material is placed in a suitable container in the form of a roll or a flat surface, and the prepared silica sol solution is injected into the laid lightweight GMT material to exhaust the air in the lightweight GMT material. After the solution is gelled, it is dried by supercritical fluid to obtain the GMT aerogel felt;
[0059] (3) Preparation of glass fiber reinforced polypropylene composite materials:
[0060] Polypropylene resin, carbon black M717, antioxidant (a mixture of the antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1) and aerogel were taken in a mass ratio of 94.5:2:0.5:3, stirred evenly at 500r / min, and melted and extruded to prepare a resin film. The resin film / glass fiber mat / resin film were laid in sequence, the molding equipment was heated to 200°C, the resin film was fully melted, hot pressed at a pressure of 5MPa, cooled and shaped, and a glass fiber mat reinforced polypropylene composite material was obtained;
[0061] (4) Hot pressing compound:
[0062] A layer of glass fiber reinforced polypropylene material composite material, a layer of aerogel reinforced GMT composite material and a glass fiber reinforced polypropylene material composite material are laid in sequence, and are compression molded by a double steel belt continuous press. The compression molding is performed at a hot pressing temperature of 200°C, a hot pressing pressure of 4 MPa and a hot pressing time of 3 minutes. The thermal insulation composite material is obtained through hot pressing composite shaping.
[0063] Example 4
[0064] (1) Preparation of lightweight GMT materials:
[0065] Polypropylene resin, polybutadiene, azobisisobutyronitrile, cyclic anhydride type and bisphenol A type cyanate were mixed in a mass ratio of 92:6:1:0.5:0.5, and then the temperature and pressure were raised to 130°C, and then the mixture was rapidly stirred at 15MPa to obtain modified polypropylene resin, which was then subjected to spinning treatment to obtain modified polypropylene fiber for use; then glass fiber and modified polypropylene fiber were selected in a mass ratio of 4:1 and mixed evenly, and then carded, laid and needled to obtain 3000g / m 2 The blended fiber felt is cut as needed for later use; the mixed powder of hydrophobic aerogel modified by kH560 and polypropylene resin powder is sprayed on the surface of the blended fiber felt at a mass ratio of 1:15 between aerogel and polypropylene resin, and the spraying amount is 100g / m 2 , a layer of mixed powder is evenly spread on its surface, and the powder is quickly impregnated into the felt by electrostatic dry impregnation, wherein the impregnation time is 15s and the travel speed is 5m / min. The mixed felt obtained above is reinforced by double-sided needle punching, and the needle punching is 50 punctures / cm up and down. 2 The needle punching depth is 15 mm up and down. The preheated felt plate is heated to 150°C and then hot-pressed for 4 minutes by continuous roller pressing. It is then placed in an oven and heated and baked at 170°C for 60 minutes to obtain a 15 mm thick lightweight GMT material.
[0066] (2) Preparation of GMT aerogel felt:
[0067] The lightweight GMT material is placed in a suitable container in the form of a roll or a flat surface, and the prepared silica sol solution is injected into the laid lightweight GMT material to exhaust the air in the lightweight GMT material. After the solution is gelled, it is dried by supercritical fluid to obtain the preparation of GMT aerogel felt;
[0068] (3) Preparation of glass fiber reinforced polypropylene composite materials:
[0069] Polypropylene resin, carbon black M717, antioxidant (a mixture of the antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1) and aerogel were taken in a mass ratio of 94.5:2:0.5:3, stirred evenly at 500r / min, and melted and extruded to prepare a resin film. The resin film / glass fiber mat / resin film were laid out in sequence after being disassembled, and the molding equipment was heated to 200°C to fully melt the resin film, hot-pressed at a pressure of 5MPa, and cooled to shape to obtain a glass fiber mat reinforced polypropylene composite material;
[0070] (4) Hot pressing compound:
[0071] A layer of glass fiber reinforced polypropylene material composite material, a layer of aerogel reinforced GMT composite material and a glass fiber reinforced polypropylene material composite material are laid in sequence, and are compression molded by a double steel belt continuous press. The compression molding is performed at a hot pressing temperature of 200°C, a hot pressing pressure of 4 MPa and a hot pressing time of 3 minutes. The thermal insulation composite material is obtained through hot pressing composite shaping.
[0072] Example 5
[0073] (1) Preparation of lightweight GMT materials:
[0074] Polypropylene resin, polybutadiene, azobisisobutyronitrile, cyclic anhydride type and bisphenol A type cyanate were mixed in a mass ratio of 92:6:1:0.5:0.5, and then the temperature and pressure were raised to 130°C, and then the mixture was rapidly stirred at 15MPa to obtain modified polypropylene resin, which was then subjected to spinning treatment to obtain modified polypropylene fiber for use; then glass fiber and modified polypropylene fiber were selected in a mass ratio of 1:2 and mixed evenly, and then carded, laid and needled to obtain 3000g / m 2 The blended fiber felt is cut as needed for later use; the mixed powder of hydrophobic aerogel modified by kH560 and polypropylene resin powder is sprayed on the surface of the blended fiber felt at a mass ratio of 1:15 between aerogel and polypropylene resin, and the spraying amount is 100g / m 2 , a layer of mixed powder is evenly spread on its surface, and the powder is quickly impregnated into the felt by electrostatic dry impregnation, wherein the impregnation time is 15s and the travel speed is 5m / min. The mixed felt obtained above is reinforced by double-sided needle punching, and the needle punching is 50 punctures / cm up and down. 2 The needle punching depth is 15 mm up and down. The preheated felt plate is heated to 150°C and then hot-pressed for 4 minutes by continuous roller pressing. It is then placed in an oven and heated and baked at 170°C for 60 minutes to obtain a 15 mm thick lightweight GMT material.
[0075] (2) Preparation of GMT aerogel felt:
[0076] The lightweight GMT material is placed in a suitable container in the form of a roll or a flat surface, and the prepared silica sol solution is injected into the laid lightweight GMT material to exhaust the air in the lightweight GMT material. After the solution is gelled, it is dried by supercritical fluid to obtain the GMT aerogel felt;
[0077] (3) Preparation of glass fiber reinforced polypropylene composite materials:
[0078] Polypropylene resin, carbon black M717, antioxidant (a mixture of the antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1) and aerogel were taken in a mass ratio of 94.5:2:0.5:3, stirred evenly at 500r / min, and melted and extruded to prepare a resin film. The resin film / glass fiber mat / resin film were laid in sequence, the molding equipment was heated to 200°C, the resin film was fully melted, hot pressed at a pressure of 5MPa, cooled and shaped, and a glass fiber mat reinforced polypropylene composite material was obtained;
[0079] (4) Hot pressing compound:
[0080] A layer of glass fiber reinforced polypropylene material composite material, a layer of aerogel reinforced GMT composite material and a glass fiber reinforced polypropylene material composite material are laid in sequence, and are compression molded by a double steel belt continuous press. The compression molding is performed at a hot pressing temperature of 200°C, a hot pressing pressure of 4 MPa and a hot pressing time of 3 minutes. The thermal insulation composite material is obtained through hot pressing composite shaping.
[0081] Example 6
[0082] (1) Preparation of lightweight GMT materials:
[0083] Polypropylene resin, polybutadiene, azobisisobutyronitrile, cyclic anhydride type and bisphenol A type cyanate were mixed in a mass ratio of 92:6:1:0.5:0.5, and then the temperature and pressure were raised to 130°C, and then the mixture was rapidly stirred at 15MPa to obtain modified polypropylene resin, which was then subjected to spinning treatment to obtain modified polypropylene fiber for use; then glass fiber and modified polypropylene fiber were selected in a mass ratio of 1:2 and mixed evenly, and then carded, laid and needled to obtain 3000g / m 2 The blended fiber felt is cut as needed for later use; the mixed powder of hydrophobic aerogel modified by kH560 and polypropylene resin powder is sprayed on the surface of the blended fiber felt at a mass ratio of 1:15 between aerogel and polypropylene resin, and the spraying amount is 100g / m 2 , a layer of mixed powder is evenly spread on its surface, and the powder is quickly impregnated into the felt by electrostatic dry impregnation, wherein the impregnation time is 15s and the travel speed is 5m / min. The mixed felt obtained above is reinforced by double-sided needle punching, and the needle punching is 50 punctures / cm up and down. 2The needle punching depth is 15 mm up and down. The preheated felt plate is heated to 150°C and then hot-pressed for 4 minutes by continuous roller pressing. It is then placed in an oven and heated and baked at 170°C for 60 minutes to obtain a 15 mm thick lightweight GMT material.
[0084] (2) Preparation of GMT aerogel felt:
[0085] The lightweight GMT material is placed in a suitable container in the form of a roll or a flat surface, and the prepared silica sol solution is injected into the laid lightweight GMT material to exhaust the air in the lightweight GMT material. After the solution is gelled, it is dried by supercritical fluid to obtain the GMT aerogel felt;
[0086] (3) Preparation of glass fiber reinforced polypropylene composite materials:
[0087] Polypropylene resin, carbon black M717, and antioxidant (a mixture of the antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1) were taken at a mass ratio of 97.5:2:0.5, stirred evenly at 500r / min, and melted and extruded to prepare a resin film. The resin film / glass fiber mat / resin film were laid in sequence, the molding equipment was heated to 200°C, the resin film was fully melted, hot pressed at a pressure of 5MPa, cooled and shaped, and a glass fiber mat reinforced polypropylene composite material was obtained;
[0088] (4) Hot pressing compound:
[0089] A layer of glass fiber reinforced polypropylene material composite material, a layer of aerogel reinforced GMT composite material and a glass fiber reinforced polypropylene material composite material are laid in sequence, and are compression molded by a double steel belt continuous press. The compression molding is performed at a hot pressing temperature of 200°C, a hot pressing pressure of 4MPa and a hot pressing time of 3min. The thermal insulation composite material is obtained through hot pressing composite shaping.
[0090] Comparative Example 1:
[0091] (1) Preparation method of common GMT composite material: glass fiber bundles are dispersed on a mesh belt, polyester resin powder is evenly sprinkled on the glass fiber bundles, and then heated to 200°C to allow the polyester resin powder to solidify to form glass fiber mat, polypropylene resin, carbon black M717, and antioxidant (a mixture of the antioxidant 1010 and the antioxidant 168 in a mass ratio of 1:1) are stirred at a speed of 1500 rpm for 5 minutes, and then melt-blended and extruded in an extruder to obtain resin matrix particles, and then the resin matrix particles are pressed into a resin matrix, and the resin matrix and a layer of glass fiber mat are alternately laid, and the equipment is heated to 230°C to fully melt the resin matrix, and hot pressed at a pressure of 10 MPa; cooled and shaped to obtain common GMT material;
[0092] (2) Mixing aerogel particles and a binder, and hot pressing to form an aerogel insulation layer. The above-mentioned common GMT material, aerogel insulation layer and common GMT material are stacked and laid in sequence.
[0093] (3) Hot pressing and shaping: The double steel belt continuous press is used for molding, the hot pressing temperature is 150°C, the hot pressing pressure is 4 MPa, and the hot pressing time is 3 min. The thermal insulation composite material is obtained by hot pressing and composite shaping.
[0094] Comparative Example 2
[0095] The difference between Comparative Example 2 and Example 1 is that in the preparation process of the lightweight GMT material, the mixed powder of resin powder and aerogel is not used for impregnation, and only a layer of resin powder is spread on the surface of the blended fiber felt.
[0096] Test Results
[0097] Test items Thermal conductivity <![CDATA[Impact strength (KJ / m 2 )]]> Peel force(N) Example 1 0.028 102 80 Example 2 0.028 105 82 Example 3 0.028 96 75 Example 4 0.035 93 74 Example 5 0.03 112 85 Example 6 0.03 107 83 Comparative Example 1 0.05 38 Layering Comparative Example 2 0.06 83 61
[0098] The embodiments of the present invention are several examples of the composite materials provided by the present invention, and the comparative examples are composite materials provided by the prior art. It can be seen from the above test results that the composite materials prepared by the present invention have excellent thermal conductivity and good mechanical properties related to impact strength and peeling force.
Claims
1. A method for preparing a thermal insulation composite material, characterized in that: The following steps are involved: (1) Preparation of lightweight GMT material: modified polypropylene fiber and glass fiber are blended to obtain a blended fiber felt, a layer of mixed powder of resin powder and hydrophobic aerogel is spread on the surface of the blended fiber felt, the mass ratio of hydrophobic aerogel to resin powder is 1:10-20, and a lightweight GMT material is obtained after impregnation, hot pressing and baking. The mixed mass ratio of modified polypropylene fiber and glass fiber is 1:
1. The preparation method of modified polypropylene fiber is as follows: 90-95 parts of polypropylene resin, 2-6 parts of polybutadiene, 0.1-1 parts of azobisisobutyronitrile, 0.1-1 parts of cyclic acid anhydride type and 0.1-1 parts of bisphenol A type cyanate are mixed, and then the temperature and pressure are increased and the mixture is rapidly stirred to obtain modified polypropylene resin, and then the modified polypropylene fiber is subjected to spin spinning treatment. The hydrophobic aerogel is an epoxy-containing aerogel prepared by surface modification of aerogel with KH560, and the resin powder is a polypropylene resin powder; (2) Preparation of GMT aerogel felt: The lightweight GMT material is impregnated and mixed with the silica sol solution, and the silica sol solution is gelled and dried to obtain the GMT aerogel felt; (3) Preparation of glass fiber reinforced polypropylene composite material: polypropylene resin, carbon black M717 and antioxidant are mixed and granulated, and then prepared into a resin film, and the resin film, glass fiber mat and resin film are laid in sequence, hot pressed and cooled to obtain a glass fiber reinforced polypropylene composite material; (4) Laying the glass fiber reinforced polypropylene composite material, the GMT aerogel felt and the glass fiber reinforced polypropylene composite material in sequence and compression molding them to obtain the thermal insulation composite material.
2. The method for preparing a thermal insulation composite material according to claim 1, characterized in that: The molding temperature in (4) is 180-200°C, the hot pressing pressure is 3-5 MPa, and the hot pressing time is 1-4 min.
3. The method for preparing a thermal insulation composite material according to claim 1, characterized in that: The thickness of GMT aerogel felt is 3~30mm, and the thickness of glass fiber reinforced polypropylene composite materials is 0.5~2mm.
4. A method for preparing a thermal insulation composite material according to any one of claims 1 to 3, characterized in that: The prepared heat insulation composite material comprises a surface layer, a core layer and a bottom layer, wherein the core layer is arranged between the surface layer and the bottom layer; The surface layer and the bottom layer are both glass fiber reinforced polypropylene composite materials; The core layer is a GMT aerogel felt, and the GMT aerogel felt includes a lightweight GMT material and an aerogel covering the surface of the lightweight GMT material; The lightweight GMT material comprises a composite layer of blended fiber felt, aerogel and resin powder, wherein the composite layer comprises two layers arranged on the upper and lower surfaces of the blended fiber felt.