A raw-ceramic composite material and a method for preparing a wafer handling arm using the same
By using green porcelain composite materials to prepare the wafer handling arm, the problems of rapid wear and vacuum leakage of existing materials are solved, higher wear resistance and vacuum reliability are achieved, and the cost of use is reduced.
Patent Information
- Application Number
- CN202310852247.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-12
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-07-12
AI Technical Summary
The materials of existing wafer handling arms wear out quickly, the use cost is high, and vacuum leaks are frequent, affecting long-term use and accuracy.
The wafer handling arm is made of green porcelain composite materials, including binders, sintering aids, plasticizers, dispersants and ceramic powders. It is molded by an isostatic press and sintered at high temperature to form a wear-resistant and sealed vacuum channel.
The wear resistance and vacuum reliability of the wafer handling arm are improved, the service life is extended, the cost is reduced, and the problem of vacuum failure is reduced.
Smart Images

Figure CN116854467B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of semiconductor wafer tools, and in particular to a raw-ceramic composite material and a method for preparing a wafer transport arm using the raw-ceramic composite material. Background Art
[0002] The chip substrate materials used in the LED industry are mainly silicon substrates, sapphire, and silicon carbide substrates. The material hardness is relatively high. They exist in the form of wafers during mass production. Conventional sizes include 4, 6, 8, 22 inches, etc. During the production and transportation process, wafers are generally inserted into cassettes for circulation processing.
[0003] The wafer box generally has a compact structure, usually about 3mm, and has extremely high requirements on the thickness of the arm. If the thickness is too large, the arm will touch the adjacent wafers during the process of taking and placing the wafers, causing collisions. Based on such thin materials, it is necessary to ensure that the vacuum arm will not deform during long-term use and will not affect the accuracy of the wafer taking position. In addition, the wafer is relatively hard, and conventional materials wear quickly and will soon be damaged, resulting in a short arm replacement cycle and high usage costs.
[0004] At present, the commonly used material of the vacuum arm is adhesive steel sheet. The steel sheet vacuum arm is composed of multiple steel sheets, which are bonded together with glue. A vacuum air channel is preset inside the arm to achieve vacuum adsorption of wafers. The steel sheet material has a low hardness and frequently rubs against the hard sapphire wafer, causing rapid wear. In addition, the adhesive steel sheets are prone to debonding and leakage during use, affecting their use. Summary of the invention
[0005] Based on this, the purpose of the present invention is to provide a raw-ceramic composite material and a method for preparing a wafer handling arm using the same, so as to solve the problems in the prior art.
[0006] On the one hand, the present invention provides a raw ceramic composite material, comprising a binder, a sintering aid, a plasticizer, a dispersant, and ceramic powder, wherein the binder comprises a P solvent and an O solvent, the P solvent has a content of 1wt%-1.5wt% and a viscosity of 60cps-70cps, the O solvent has a content of 3wt%-6.5wt% and a viscosity of not less than 4800cps, the sintering aid has a content of 3.5wt%-5wt%, the plasticizer has a content of 2wt%-10wt%, the dispersant has a content of 2wt%-4wt%, and the rest is ceramic powder.
[0007] Preferably, the ceramic powder includes one or more of a first zirconia powder having a particle size of 0.4 μm-0.48 μm, a second zirconia powder having a particle size of 0.65 μm-0.75 μm, and a third zirconia powder having a particle size of 0.95 μm-1.1 μm.
[0008] Another aspect of the present invention provides a method for preparing a wafer handling arm using the green ceramic composite coil, comprising the following steps:
[0009] Using the green ceramic composite material to prepare a green ceramic sheet;
[0010] Selecting the green ceramic sheets according to a preset number to form a green ceramic sheet group, placing the green ceramic sheet group in a stacking box, and performing isostatic pressing and stacking by an isostatic press to prepare a semi-finished product structural layer;
[0011] The semi-finished product structure layer is laser-drilled and cut according to a preset structure shape to form a first structure layer, a second structure layer, a third structure layer and a fourth structure layer of different shapes, wherein the second structure layer is provided with a plurality of vacuum holes for adsorbing wafers, and the third structure layer is provided with a vacuum flow channel connected with the vacuum hole;
[0012] The fourth structural layer, the third structural layer, the second structural layer and the first structural layer are sequentially mounted on a lamination table, and are subjected to lamination and static pressing treatment by an isostatic press to form the layers into one piece, thereby obtaining a semi-finished transport arm;
[0013] The semi-finished wafer handling arm is placed in a vacuum sintering furnace for sintering to obtain a finished wafer handling arm.
[0014] Preferably, the process of preparing a green ceramic sheet using the green ceramic composite material specifically comprises:
[0015] Putting the raw porcelain composite material into a vacuum stirring tank for vacuum stirring and mixing, removing bubbles in the raw porcelain composite material, and obtaining a casting slurry;
[0016] The casting slurry is subjected to a casting process by a casting roller to prepare a green porcelain coil having a uniform thickness, wherein the casting process temperature is 30° C.-65° C., the casting speed is 3 m / min-5 m / min, and the thickness of the prepared green porcelain coil is 150 μm-155 μm;
[0017] The green porcelain coil is cut to obtain the green porcelain sheets.
[0018] Preferably, the preset number is 4 or 5 pieces.
[0019] Preferably, placing the green ceramic sheet group into a stacking box for static pressing stacking to prepare the semi-finished product structure layer specifically includes:
[0020] Arranging a PET film at the bottom of the stacking box, and periodically and cross-arranging the green ceramic sheet group and the PET film on the PET film until it is flush with the top opening of the stacking box;
[0021] Putting the stacking box in which the green ceramic sheet group and the PET film are arranged into an isostatic press mold for isostatic pressing;
[0022] After static pressing, each of the green ceramic sheets in the green ceramic sheet group is integrally formed, and the integrally formed green ceramic sheet group is separated by the PET film to obtain the semi-finished product structural layer.
[0023] Preferably, the step of sequentially placing the fourth structural layer, the third structural layer, the second structural layer and the first structural layer on a lamination table specifically comprises:
[0024] The first structural layer, the second structural layer, the third structural layer and the fourth structural layer are all provided with fixing holes, and the stacking platform is provided with positioning pins matched with the fixing holes;
[0025] The fourth structural layer and the third structural layer are sequentially sleeved on the lamination table through the fixing holes and the positioning pins, and the vacuum flow channel is filled, and the filler in the vacuum flow channel melts and evaporates during the sintering process;
[0026] The second structural layer and the first structural layer are sequentially sleeved on the lamination table through the fixing holes and the positioning pins, and the top of the positioning pins is higher than the first structural layer.
[0027] Preferably, the isostatic pressing of the sheets to form the semi-finished transport arm in one piece comprises:
[0028] Arranging and fixing a rubber strip on the positioning pins higher than the first structural layer;
[0029] Put the fixed stacking table into a vacuum bag, evacuate the vacuum bag and seal it, and check whether the vacuum bag leaks after standing for a preset time;
[0030] If there is no leakage in the vacuum bag, place the vacuum bag in the container of the isostatic press for isostatic pressure treatment at a pressure of 50 kg / cm 2 -300kg / cm 2 , the liquid temperature in the isostatic press container is 80℃-85℃, and the static pressing time is 20min-30min;
[0031] After the isostatic pressing is completed, the vacuum bag is taken out from the isostatic press, and the vacuum bag is opened to take out the one-piece semi-finished handling arm.
[0032] Preferably, the step of placing the semi-finished wafer handling arm into a vacuum sintering furnace for sintering to obtain a finished wafer handling arm specifically includes:
[0033] Placing the semi-finished product transporting arm on the sintering plate, and placing a smoothing plate above the semi-finished product transporting arm;
[0034] Place spacers around the sintering plate, and place the sintering plate, the semi-finished product transport arm, and the smoothing plate on the spacers in sequence, and cycle in sequence to form a plurality of semi-finished product transport arms stacked at intervals;
[0035] Place a dust cover on the topmost smoothing plate, transfer the semi-finished product handling arms stacked at intervals into a vacuum sintering furnace, gradually increase the temperature in the sintering furnace to 1600°C-1650°C, keep it warm for 4h-6h, and finally gradually cool it down to 40°C-50°C to obtain a finished wafer handling arm.
[0036] Preferably, the preparation method further comprises:
[0037] Grinding the surface of the finished wafer transfer arm to remove burrs, and blowing and cleaning the vacuum chamber to remove impurities in the vacuum chamber;
[0038] Grinding the adsorption surface provided with the vacuum hole to clean off the surface grinding powder;
[0039] A polishing liquid is prepared, wherein the polishing liquid is a mixture of aluminum oxide powder and water, and the mass ratio of the aluminum oxide powder to water is 1:10;
[0040] The polishing liquid is used to polish the ground adsorption surface, and the roughness of the polished adsorption surface is within Ra0.1
[0041] The invention has the following beneficial effects: providing a raw porcelain composite material formula, the raw porcelain sheet prepared by the raw porcelain composite material is easy to process, laser cutting is less difficult to process, has a high yield rate and low comprehensive processing cost compared with traditional hard processing; the vacuum reliability of the handling arm is better through the one-piece molding process of the isostatic press, and no stratification or air leakage will occur during long-term use; after high-temperature sintering, the surface oxidation resistance of the wafer handling arm is significantly better than that of the metal material, the Mohs hardness of the zirconia ceramic surface can reach 7.5-8.0, the adsorption position has strong wear resistance, and the vacuum failure problem caused by wear and deformation of the adsorption position is reduced, which has obvious advantages over the traditional steel sheet bonding type; in addition, the overall thickness of the wafer handling arm prepared by the present application is relatively thin, generally about 2 mm, which meets the thickness requirement limit of the pick-and-place sheet, and reduces the risk of collision with upper and lower adjacent wafers; further, different structural layers are prepared by the preparation method of the present application, and the second structural layer and the fourth structural layer are placed above and below the third structural layer, respectively, to form a sealed vacuum air duct, and the vacuum air duct is inside the handling arm, which reduces the problem of air leakage caused by debonding and stratification of traditional steel sheets.
[0042] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 A flow chart of a method for preparing a wafer handling arm provided by the present invention;
[0044] Figure 2 It is a schematic diagram of statically pressing and laminating green ceramic sheets of the present invention;
[0045] Figure 3 It is a schematic diagram of the structure of each structural layer of the present invention;
[0046] Figure 4 It is a schematic diagram of static pressure lamination of the structural layer of the present invention;
[0047] Figure 5 It is a schematic diagram of the stacking structure of the semi-finished product transport arm in the sintering process of the present invention.
[0048] Description of main component symbols:
[0049] 10. Stacking box; 11. Raw ceramic sheet; 12. PET film; 20. Stacking table; 21. First structural layer; 22. Second structural layer; 23. Third structural layer; 24. Fourth structural layer; 25. Fixing hole; 26. Vacuum hole; 27. Vacuum flow channel; 30. Semi-finished product handling arm; 31. Sintering plate; 32. Smoothing plate; 33. Spacer; 34. Dust cover.
[0050] The following specific implementation manner will further illustrate the present invention in conjunction with the above-mentioned drawings. DETAILED DESCRIPTION
[0051] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. Several embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thorough and comprehensive.
[0052] It should be noted that when an element is referred to as being "fixed to" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only.
[0053] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0054] The present invention provides a raw ceramic composite material, comprising a binder, a sintering aid, a plasticizer, a dispersant, and ceramic powder, wherein the binder comprises a P solvent and an O solvent, the content of the P solvent is 1wt%-1.5wt% and the viscosity is 60cps-70cps, the content of the O solvent is 3wt%-6.5wt% and the viscosity is not less than 4800cps, the content of the sintering aid is 3.5wt%-5wt%, the content of the plasticizer is 2wt%-10wt%, the content of the dispersant is 2wt%-4wt%, and the rest is ceramic powder, it should be understood that the above contents are calculated by weight; specifically, in the present embodiment, the ceramic powder comprises one or more of a first zirconium oxide powder with a particle size of 0.4μm-0.48μm, a second zirconium oxide powder with a particle size of 0.65μm-0.75μm, and a third zirconium oxide powder with a particle size of 0.95μm-1.1μm.
[0055] Embodiment 1
[0056] The first embodiment of the present invention provides a method for preparing a wafer handling arm using the above-mentioned green ceramic composite coil material, such as Figure 1 As shown, the preparation method comprises the following steps:
[0057] S10, preparing a green ceramic sheet using the green ceramic composite material;
[0058] Optionally, in the present embodiment, in the raw porcelain composite material, the content of P solvent is 1wt%, and the viscosity is 65cps; the content of O solvent is 5wt%, and the viscosity is 4800cps; the content of sintering aid is 3.5wt%, the content of plasticizer is 2wt%, and the plasticizer can improve the strength of the raw porcelain composite material; the content of dispersant is 2wt%, and the dispersant can improve the mixing uniformity of the powder; the rest is ceramic powder, wherein the ceramic powder includes a first zirconium oxide powder with a particle size of 0.4μm, a second zirconium oxide powder with a particle size of 0.65μm and a third zirconium oxide powder with a particle size of 0.95μm, and the ceramic powder is dried at a drying temperature of 125℃-135℃ and a drying time of 22h-26h. Preferably, in the present embodiment, the drying temperature is 130℃ and the drying time is 24h.
[0059] In the specific implementation, the raw porcelain composite material in this embodiment is placed in a vacuum stirring tank for vacuum stirring and mixing, the speed of the vacuum stirring tank is set to 12RPM-16RPM (RPM: Revolutions Per Minute, revolutions per minute), and the stirring time is 4h-6h. Preferably, in this embodiment, the speed of the vacuum stirring tank is set to 15RPM and the stirring time is 5h. During the stirring process, the vacuum stirring tank is evacuated to remove bubbles in the raw porcelain composite material to obtain a high-viscosity casting slurry. The casting slurry is cast by a casting roller to prepare a raw porcelain coil with uniform thickness, wherein the casting temperature is 30℃-65℃, the casting speed is 3m / min-5m / min, and the thickness of the prepared raw porcelain coil is 150μm-155μm. Preferably, the casting temperature is 40℃, the casting speed is 4m / min, and the thickness of the prepared raw porcelain coil is 150μm. The raw porcelain coil is cut to obtain raw porcelain sheets. In the specific implementation, when the raw porcelain coil is prepared, the raw porcelain coil is placed on a cutting machine for cutting to obtain a number of raw porcelain sheets. Since the wafer handling arm prepared from the raw porcelain composite material provided by the present invention will shrink during high-temperature sintering (the shrinkage is generally 73%-80%), optionally, in this embodiment, the length of the cut raw porcelain sheet generally exceeds the calculated length, for example, it can exceed 5-10mm as needed.
[0060] S20, selecting the green ceramic sheets according to a preset number to form a green ceramic sheet group, placing the green ceramic sheet group into a stacking box, and performing isostatic pressing and stacking by an isostatic press to prepare a semi-finished product structural layer;
[0061] During specific implementation, the number of raw ceramic sheets is selected according to actual needs and design requirements. For example, the number of raw ceramic sheets can be selected according to the designed thickness to form a raw ceramic sheet group, and subsequent static pressure lamination is performed to prepare a semi-finished structural layer. Optionally, the number of raw ceramic sheets in the semi-finished structural layer is 4 or 5. Specifically, in order to improve the efficiency of preparing the semi-finished structural layer, multiple raw ceramic sheet groups can be laminated simultaneously.
[0062] In specific implementation, Figure 2 As shown, the size of the stacking box 10 is larger than the outer width of the raw ceramic sheet 11 by 0.5mm-0.8mm. First, the PET film 12 is arranged at the bottom of the stacking box 10, and then the raw ceramic sheet groups and the PET film are periodically arranged crosswise on the PET film at the bottom until it is flush with the top opening of the stacking box. The bottom and top of the stacking box are both PET films; so that each raw ceramic sheet group is separated by the PET film to prevent the raw ceramic sheets between different raw ceramic sheet groups from sticking together during static pressure, which is conducive to the separation of different semi-finished product structural layers. In another optional embodiment, the height inside the stacking box can also be slightly higher or lower than the top opening of the stacking box. Preferably, the distance above or below the top opening does not exceed 1.5mm.
[0063] Put the stacking box with the green ceramic sheet group and PET film arranged into the isostatic press mold for static pressure treatment; in the specific implementation, put the stacking box with the green ceramic sheet group and PET film arranged into a vacuum bag, evacuate the vacuum bag and seal the mouth of the vacuum bag, let it stand for more than 5 minutes, and check whether the vacuum bag has any air leakage. Normal vacuum packaging keeps the vacuum bag tightly contracted after standing. If the vacuum bag has air leakage, it can be seen that the packaging bag is loose after standing, and gas enters the packaging bag. After checking that the vacuum bag has no air leakage, put it into the closed container of the isostatic press for static pressure treatment. The liquid pressure of the static pressure can be 50kg / cm 2 -300kg / cm 2 The temperature of the liquid is 75°C-85°C, the static pressure time is 20min-30min, and optionally, in this embodiment, the static pressure of the liquid can be 100kg / cm 2 , the temperature of the liquid is 80℃, the static pressing time is 25min, and the green ceramic sheets are subjected to the same pressure through the isostatic press. After the static pressing is completed, take it out of the static press, wipe the liquid on the surface of the packaging bag, and then open the vacuum bag; after static pressing, each green ceramic sheet in each green ceramic sheet group is pressed and formed into one piece, and the green ceramic sheet group after the one-piece forming is separated by the PET film to obtain several semi-finished product structure layers.
[0064] S30, laser drilling and cutting are performed on the semi-finished structural layer according to a preset structural shape to form a first structural layer, a second structural layer, a third structural layer and a fourth structural layer of different shapes, wherein the second structural layer is provided with a plurality of vacuum holes for adsorbing wafers, and the third structural layer is provided with a vacuum flow channel connected to the vacuum hole.
[0065] In specific implementation, Figure 3 As shown, the semi-finished structural layer is laser cut and laser punched according to a preset structural shape. Specifically, in the present embodiment, each semi-finished structural layer can be equally divided into four areas, and each area is punched and cut by laser to prepare a first structural layer 21, a second structural layer 22, a third structural layer 23 and a fourth structural layer 24 of different shapes, that is, four structural layers can be prepared on a semi-finished structural layer at the same time, and the second structural layer is provided with a plurality of vacuum holes, and the adsorption surface with the vacuum holes is used for adsorbing wafers to complete the transfer of the wafers, and the third structural layer is provided with a vacuum flow channel connected to the vacuum hole, and the vacuum flow channel is connected to the vacuum pumping equipment, so that the adsorption surface with the vacuum holes generates negative pressure suction.
[0066] S40, sequentially mounting the fourth structural layer, the third structural layer, the second structural layer and the first structural layer on a lamination table, and laminating and isostatically pressing the layers through an isostatic press to form the layers into one piece, thereby obtaining a semi-finished transport arm.
[0067] like Figure 3 and Figure 4 As shown, a plurality of positioning pins are provided on the lamination table 20. Optionally, the first structural layer 21 includes a fixing portion and a connecting portion, the fixing portion is a square fixing portion, the connecting portion is a long strip connecting portion, and the fixing portion and the connecting portion are both provided with a plurality of fixing holes 25. The second structural layer 22 includes a fixing portion, a connecting portion and a clamping portion, the clamping portion is a "U"-shaped clamping portion, and a plurality of vacuum holes 26 are symmetrically provided on the clamping portion of the second structural layer 22, and the vacuum holes are symmetrically arranged on both sides of the axis of the "U"-shaped clamping portion. The third structural layer 23 includes a fixing portion, a connecting portion and a clamping portion, and a vacuum flow channel 27 extending from the fixing portion to the clamping portion is provided on the third structural layer 23, and the vacuum flow channel 27 is arc-shaped at the clamping portion; Preferably, the vacuum channel 27 is a groove running through the third structural layer 23, and the upper and lower ends of the groove are in contact with the second structural layer 22 and the third structural layer 23 respectively to form a vacuum air channel; the fourth structural layer 24 includes a fixing part, a connecting part and a clamping part; preferably, the fixing part and the connecting part of the first structural layer 21, the second structural layer 22, the third structural layer 23, and the fourth structural layer 24 have the same shape, and the shape and inner diameter of the fixing holes arranged on the respective fixing parts and connecting parts are also the same, and the shape of the clamping part of the second structural layer 22, the third structural layer 23, and the fourth structural layer 24 is the same. Preferably, in order to improve the static pressure stability of each structural layer, fixing holes are also provided on both sides of the opening end of the clamping part. The shape and number of each fixing hole are adapted to the positioning pins on the stacking table 20.
[0068] The cut first structural layer 21, second structural layer 22, third structural layer 23, and fourth structural layer 24 are stacked according to the designed structure. During the stacking process, the fixing holes of each structural layer are aligned with the positioning pins on the stacking table 20 and completely pressed into place. Specifically, first, the fixing holes on the fourth structural layer 24 are aligned with the positioning pins on the stacking table, and the fourth structural layer 24 is placed on the stacking table 20. Similarly, the third structural layer 23 is then placed on the stacking table 20, and the vacuum flow channel 27 is filled. The size of the filler is slightly smaller than that of the vacuum flow channel 27. The filler will melt and evaporate during the sintering process to prevent the vacuum air channel from being blocked after static pressure, and to keep the vacuum air channel of the transport arm unobstructed after sintering. Finally, the second structural layer and the first structural layer are successively sleeved on the stacking table through the fixing holes and the positioning pins. After the first structural layer is placed in, the top of the positioning pin is 0.5mm-1mm higher than the first structural layer.
[0069] A rubber strip is placed at the corresponding position on the upper surface of the positioning pin higher than the first structural layer, and masking tape is used to assist in fixing to prevent the raised positioning pin from piercing the vacuum bag. The stacking table 20 with the structural layer is placed in the vacuum bag, the vacuum bag is evacuated and the mouth of the vacuum bag is sealed. The bag is left to stand for more than 5 minutes, and the vacuum bag is checked for air leakage. Normal vacuum packaging keeps the vacuum bag tightly contracted after standing. If the vacuum bag has air leakage, the bag can be visually seen to be loose after standing, and gas enters the bag. After checking that the vacuum bag has no air leakage, it is placed in a closed container of an isostatic press for static pressure treatment. The liquid pressure of the static pressure can be 50kg / cm 2 -300kg / cm 2 The temperature of the liquid is 75°C-85°C, the static pressure time is 20min-30min, and optionally, in this embodiment, the static pressure of the liquid can be 120kg / cm 2 , the temperature of the liquid is 80°C, the static pressing time is 25 minutes, and each structural layer is subjected to the same pressure through the isostatic press. After the static pressing is completed, it is taken out from the static press, and the liquid on the surface of the packaging bag is wiped dry. After the static pressing, each structural layer is integrally formed, and then the vacuum bag is disassembled; the semi-finished handling arm 30 is obtained.
[0070] S50, placing the semi-finished wafer handling arm into a vacuum sintering furnace for sintering to obtain a finished wafer handling arm.
[0071] In specific implementation, Figure 5 As shown, the semi-finished product conveying arm 30 after static pressing is placed on the sintering plate 31. Preferably, in order to improve the sintering efficiency, multiple semi-finished product conveying arms can be placed on the sintering plate in parallel, with each semi-finished product conveying arm spaced 5mm-10mm apart, and then a caressing plate 32 is placed above the semi-finished product conveying arms placed in parallel; spacers 33 are placed around the sintering plate, and the sintering plate, the semi-finished product conveying arm, and the caressing plate are placed on the spacers 33 in sequence, and the cycle is repeated in sequence to form a plurality of semi-finished product conveying arms stacked at intervals; During the sintering process, the temperature field on the surface of the product is uniform and the heat is uniformly received. A dust cover plate 34 is placed on the topmost smoothing plate 32. Finally, the stacked semi-finished product handling arms are transferred to the vacuum sintering furnace. The temperature in the sintering furnace is gradually increased to 1600°C-1650°C. Optionally, the temperature can be gradually increased at a heating rate of 3°C / min. After the temperature reaches 1600°C-1650°C, it is kept warm for 4h-6h and finally gradually cooled to 40°C-50°C to obtain a finished wafer handling arm.
[0072] The raw porcelain composite material and the wafer handling arm prepared by using the composite material provided by the present application provide a raw porcelain composite material formula. The raw porcelain sheet prepared by the raw porcelain composite material is easy to process. Compared with traditional hard processing, laser cutting has less processing difficulty, higher yield rate and lower comprehensive processing cost. The vacuum reliability of the handling arm is improved by the one-piece molding process of the isostatic press, and no delamination or air leakage will occur during long-term use. After high-temperature sintering, the surface oxidation resistance of the wafer handling arm is significantly better than that of metal materials. The Mohs hardness of the zirconia ceramic surface can reach 7.5-8.0, and the adsorption position has strong wear resistance, which reduces the vacuum failure problem caused by wear and deformation of the adsorption position. Compared with the traditional steel sheet bonding type, it has obvious advantages. In addition, the overall thickness of the wafer handling arm prepared by the present application is relatively thin, generally about 2 mm, which meets the thickness requirement limit for picking and placing wafers and reduces the risk of colliding with upper and lower adjacent wafers; further, different structural layers are prepared by the preparation method of the present application, and the second structural layer and the fourth structural layer are respectively placed above and below the third structural layer to form a sealed vacuum air duct. The vacuum air duct is inside the handling arm to reduce the problem of air leakage caused by debonding and stratification of traditional steel sheets. When used specifically, the vacuum extraction device evacuates the vacuum air duct of the third structural layer, and transmits the vacuum suction to the surface of the wafer through the vacuum hole connected to the vacuum air duct to absorb the wafer.
[0073] Embodiment 2
[0074] The difference between the method for preparing the wafer transport arm in this embodiment and the method for preparing the wafer transport arm in the first embodiment is that the method for preparing the wafer transport arm further comprises:
[0075] Grinding the surface of the finished wafer handling arm to remove burrs, and performing air blowing cleaning to remove impurities in the vacuum flow channel;
[0076] During the specific implementation, the surface of the sintered handling arm is polished to remove burrs, and is checked for deformation, delamination, etc. It is checked whether the shape tolerance, flatness and other parameters of the finished wafer handling arm are within the tolerance range. The surface of the product is cleaned, the vacuum air duct is blown and cleaned to remove dust and impurities in the middle, and a test is conducted for leaks.
[0077] Grinding the adsorption surface with vacuum holes to clean the surface grinding powder;
[0078] In the specific implementation, the second structural layer and the clamping part are provided with a plurality of through vacuum holes. One side of the clamping part of the second structural layer is connected to the third structural layer, and the vacuum hole is connected to the vacuum airway. The other side is an adsorption surface for adsorbing the wafer under the action of vacuum suction. In order to improve the adsorption effect, the adsorption surface is ground to improve the flatness. Specifically, the adsorption surface of the transport arm is facing up and fixed on the grinding workbench. The adsorption surface is ground with a grinding wheel. The feed rate is 0.005mm / min and the removal amount is 30um-40um until the entire adsorption surface is ground. Finally, the grinding powder on the surface is rinsed off.
[0079] Prepare a polishing liquid, which is a mixture of aluminum oxide powder and water, with a mass ratio of aluminum oxide powder to water of 1:10;
[0080] The ground adsorption surface is polished with a polishing liquid, and the roughness of the polished adsorption surface is within Ra0.1.
[0081] In the specific implementation, the transport arm is fixed on the workbench of the polishing machine with the adsorption surface facing upward. Alumina polishing liquid is used, the nozzle is opened, and the ground adsorption surface is polished. The polishing head speed is 300RPM, the downward feed rate is set to 0.001mm / min, the removal amount is 8um-10um, and the surface roughness after polishing reaches within RA0.1. There are no obvious unpolished marks or visible scratches. After all are qualified, the finished transport arm after grinding and polishing is obtained.
[0082] Embodiment 3
[0083] The difference between the raw ceramic composite material for preparing the wafer handling arm in this embodiment and that in the first embodiment is that:
[0084] In this embodiment, the content of P solvent is 1.5wt% and the viscosity is 60cps, the content of O solvent is 3wt% and the viscosity is 5000cps, the content of sintering aid is 4wt%, the content of plasticizer is 5wt%, the content of dispersant is 3wt%, and the rest is ceramic powder, which includes a first zirconium oxide powder with a particle size of 0.45μm, a second zirconium oxide powder with a particle size of 0.7μm and a third zirconium oxide powder with a particle size of 1μm.
[0085] Embodiment 4
[0086] The difference between the raw ceramic composite material for preparing the wafer handling arm in this embodiment and that in the first embodiment is that:
[0087] In this embodiment, the content of P solvent is 1.25wt%, the viscosity is 70cps, the content of O solvent is 6.5wt%, the viscosity is 5200cps, the content of sintering aid is 5wt%, the content of plasticizer is 10wt%, the content of dispersant is 4wt%, and the rest is ceramic powder, which includes a first zirconium oxide powder with a particle size of 0.48μm, a second zirconium oxide powder with a particle size of 0.5μm and a third zirconium oxide powder with a particle size of 1.1μm.
[0088] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0089] The above embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present invention. It should be pointed out that, for a person of ordinary skill in the art, several modifications and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the present invention patent shall be subject to the attached claims.
Claims
1. A method for preparing a wafer transport arm, characterized in that: The following steps are involved: A green ceramic sheet is prepared by using a green ceramic composite material; Selecting the green ceramic sheets according to a preset number to form a green ceramic sheet group, placing the green ceramic sheet group in a stacking box, and performing isostatic pressing and stacking by an isostatic press to prepare a semi-finished product structural layer; The semi-finished product structure layer is laser-drilled and cut according to a preset structure shape to form a first structure layer, a second structure layer, a third structure layer and a fourth structure layer of different shapes, wherein the second structure layer is provided with a plurality of vacuum holes for adsorbing wafers, and the third structure layer is provided with a vacuum flow channel connected with the vacuum hole; The fourth structural layer, the third structural layer, the second structural layer and the first structural layer are sequentially mounted on a lamination table, and are subjected to lamination and static pressing treatment by an isostatic press to form the layers into one piece, thereby obtaining a semi-finished transport arm; placing the semi-finished wafer handling arm into a vacuum sintering furnace for sintering to obtain a finished wafer handling arm; The step of sequentially placing the fourth structural layer, the third structural layer, the second structural layer and the first structural layer on the lamination table specifically includes: The first structural layer, the second structural layer, the third structural layer and the fourth structural layer are all provided with fixing holes, and the stacking platform is provided with positioning pins matched with the fixing holes; The fourth structural layer and the third structural layer are sequentially sleeved on the lamination table through the fixing holes and the positioning pins, and the vacuum flow channel is filled, and the filler in the vacuum flow channel melts and evaporates during the sintering process; The second structural layer and the first structural layer are sequentially sleeved on the lamination table through the fixing holes and the positioning pins, and the top of the positioning pins is higher than the first structural layer; The raw ceramic composite material comprises: a binder, a sintering aid, a plasticizer, a dispersant, and ceramic powder, wherein the binder comprises a P solvent and an O solvent, the P solvent has a content of 1wt%-1.5wt% and a viscosity of 60cps-70cps, the O solvent has a content of 3wt%-6.5wt% and a viscosity of not less than 4800cps, the sintering aid has a content of 3.5wt%-5wt%, the plasticizer has a content of 2wt%-10wt%, the dispersant has a content of 2wt%-4wt%, and the rest is ceramic powder; the ceramic powder comprises one or more of a first zirconium oxide powder having a particle size of 0.4μm-0.48μm, a second zirconium oxide powder having a particle size of 0.65μm-0.75μm, and a third zirconium oxide powder having a particle size of 0.95μm-1.1μm; The method of using the green ceramic composite material to prepare a green ceramic sheet specifically includes: Putting the raw porcelain composite material into a vacuum stirring tank for vacuum stirring and mixing, removing bubbles in the raw porcelain composite material, and obtaining a casting slurry; The casting slurry is subjected to a casting process by a casting roller to prepare a green porcelain coil having a uniform thickness, wherein the casting process temperature is 30° C.-65° C., the casting speed is 3 m / min-5 m / min, and the thickness of the prepared green porcelain coil is 150 μm-155 μm; Cutting the raw porcelain coil to obtain the raw porcelain sheets; The isostatic press is used to perform isostatic pressing on the sheets to form the semi-finished transport arm into one piece, and the semi-finished transport arm specifically comprises: Arranging and fixing a rubber strip on the positioning pins higher than the first structural layer; Put the fixed stacking table into a vacuum bag, evacuate the vacuum bag and seal it, and check whether the vacuum bag leaks after standing for a preset time; If there is no leakage in the vacuum bag, place the vacuum bag in the container of the isostatic press for isostatic pressure treatment at a pressure of 50 kg / cm 2 -300kg / cm 2 , the liquid temperature in the isostatic press container is 80℃-85℃, and the static pressing time is 20min-30min; After the isostatic pressing is completed, the vacuum bag is taken out from the isostatic press, and the vacuum bag is opened to take out the one-piece semi-finished handling arm; The step of placing the semi-finished wafer handling arm into a vacuum sintering furnace for sintering to obtain a finished wafer handling arm specifically includes: Placing the semi-finished product transporting arm on the sintering plate, and placing a smoothing plate above the semi-finished product transporting arm; Place spacers around the sintering plate, and place the sintering plate, the semi-finished product transport arm, and the smoothing plate on the spacers in sequence, and cycle in sequence to form a plurality of semi-finished product transport arms stacked at intervals; Place a dust cover on the topmost smoothing plate, transfer the semi-finished product handling arms stacked at intervals into a vacuum sintering furnace, gradually increase the temperature in the sintering furnace to 1600°C-1650°C, keep it warm for 4h-6h, and finally gradually cool it down to 40°C-50°C to obtain a finished wafer handling arm.
2. The method for preparing a wafer transport arm according to claim 1, characterized in that: The preset number is 4 or 5 pieces.
3. The method for preparing a wafer transport arm according to claim 1, characterized in that: The step of placing the green ceramic sheet group into a stacking box for static pressing and stacking to prepare a semi-finished product structure layer specifically includes: Arranging a PET film at the bottom of the stacking box, and periodically and cross-arranging the green ceramic sheet group and the PET film on the PET film until it is flush with the top opening of the stacking box; Putting the stacking box in which the green ceramic sheet group and the PET film are arranged into an isostatic press mold for isostatic pressing; After static pressing, each of the green ceramic sheets in the green ceramic sheet group is integrally formed, and the integrally formed green ceramic sheet group is separated by the PET film to obtain the semi-finished product structural layer.
4. The method for preparing a wafer transport arm according to claim 1, characterized in that: The preparation method further comprises: Grinding the surface of the finished wafer handling arm to remove burrs, and performing air blowing cleaning to remove impurities in the vacuum flow channel; Grinding the adsorption surface provided with the vacuum hole to clean off the surface grinding powder; A polishing liquid is prepared, wherein the polishing liquid is a mixture of aluminum oxide powder and water, and the mass ratio of the aluminum oxide powder to water is 1:10; The polishing liquid is used to polish the ground adsorption surface, and the roughness of the polished adsorption surface is within Ra0.1.
Citation Information
Patent Citations
Ceramics substrate preparation method
CN102745995A
Aluminum oxide ceramic substrate with high heat conductivity and preparation method thereof
CN103408291A
Hand-held terminal product appearance ceramic thin type member and production method thereof
CN104844198A
Tape casting method for zirconium oxide ceramic
CN107986780A
Nitride ceramic tape casting slurry and nitride ceramic substrate prepared from the same
CN111747756A