A magnesium ammonium phosphate-based steel substrate anticorrosion coating and preparation method thereof

By combining specific proportions of ammonium phosphate adhesive and other components in the anticorrosion coating of ammonium phosphate-based steel substrate, the problems of harsh construction conditions and slow curing speed of inorganic adhesive coating are solved, and rapid curing is achieved at room temperature and high-strength coatings improve the adhesion and corrosion resistance of the coating, ensuring long-term stability and easy transportation and storage.

CN116855108BActive Publication Date: 2024-11-05SANJIANG UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310616083.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-29
Publication Date
2024-11-05
Estimated Expiration
2043-05-29

AI Technical Summary

Technical Problem

The existing inorganic adhesive coatings have harsh construction conditions, low-temperature film formation, slow curing speed, easy volume shrinkage during curing, phosphate anti-corrosion coatings need to be baked at high temperature to cure, inconvenient for transportation and storage, too fast settling time and inconvenient for construction , the long-term water stability of the coating hardened body is insufficient.

Method used

The anticorrosion coating of ammonium phosphate-based steel substrate is used to mix ammonium phosphate adhesive, retarder, defoaming agent, corrosion inhibition and toughening components in a specific proportion, and prepare the coating slurry by using a dry powder stirring mechanism. , spray or brush at room temperature to form an anticorrosion coating with a dense structure, with fast hardness, high strength, volume stability and good water stability.

Benefits of technology

It realizes rapid curing and high-strength coatings for construction at room temperature, avoids the need for high-temperature baking, improves the adhesion, corrosion resistance and toughness of the coating, ensures the long-term stability of the coating and is easy to transport and preserve.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116855108B_ABST
    Figure CN116855108B_ABST
Patent Text Reader

Abstract

The present application discloses a magnesium ammonium phosphate-based steel substrate anticorrosion coating and a preparation method thereof, wherein dead burnt magnesium oxide powder, metakaolin and / or sulphoaluminate cement, and borax are stirred and mixed as component A, ammonium dihydrogen phosphate, boric acid, aluminum tripolyphosphate and its modified products, and carboxymethyl chitosan are stirred and mixed as component B, and polyether-modified polysiloxane and basic magnesium sulfate whisker are mixed as component C; the dry powders of components A and B are mixed with water under a natural environment, component C is added and stirred again to obtain magnesium ammonium phosphate-based steel substrate anticorrosion coating slurry; the magnesium ammonium phosphate-based steel substrate anticorrosion coating is a three-component solid powder, which is easy to store. The coating slurry preparation process is simple and can be constructed at room temperature. The slurry can ensure good workability within 20-50 minutes, and steel facilities can be easily applied and repaired for a second time at the construction site. After the construction is completed, the coating can be cured autonomously under normal atmospheric conditions to avoid the need for special curing equipment and heating processes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of anti-corrosion coatings, and in particular to a magnesium ammonium phosphate-based steel substrate anti-corrosion coating and a preparation method thereof. Background Art

[0002] Steel is an important raw material in industrial development and is widely used in construction, transportation, machinery manufacturing and other fields. Applying anti-corrosion coatings on the surface of steel is one of the most effective ways to prevent corrosion of steel facilities. The main adhesive of the anti-corrosion coating has a key impact on its performance. Among them, inorganic adhesive coatings themselves do not release toxic gases and age, which is more advantageous than organic adhesive coatings. However, most inorganic adhesive coatings have defects such as harsh construction conditions, low-temperature film formation, slow curing speed, easy volume shrinkage during the curing process, and brittle coatings, which limit their scope of use.

[0003] In the inorganic adhesive coating system, silicate adhesives and phosphate adhesives are mainly used. Compared with silicate adhesive coatings, high temperature resistant and anti-corrosion coatings based on phosphate adhesives have better performance in all aspects, especially in terms of adhesion. The phosphating treatment of steel, which is widely used at present, is a common surface treatment technology for steel. The principle is that the iron element on the surface of the steel will react with phosphate to form an iron phosphate protective film to protect the steel. This chemical reaction can also improve the bonding force between the steel substrate and the phosphate coating, making the coating more adherent to the steel substrate. The existing phosphate heat-resistant coatings have attracted widespread attention due to their advantages of strong adhesion, good high temperature resistance, low price, low toxicity, less pollution, non-flammable and non-explosive. However, some phosphate anti-corrosion coatings disclosed in the prior art must be baked at a higher temperature to achieve solidification, resulting in their failure to be widely promoted and applied.

[0004] The magnesium phosphate adhesive can be hardened and solidified at room temperature by mixing with water to form a dense structure similar to sintered ceramics, and has excellent properties such as fast hardening, high strength, low shrinkage, anti-freezing and salt freezing, anti-salt erosion, high temperature resistance and strong environmental adaptability. There have been some public reports on the preparation of coating materials using magnesium phosphate adhesives.

[0005] CN 106116438 B provides a magnesium phosphate-based steel bar protective coating material and a preparation method thereof. The coating material is presented in component A and component B. Component B needs to be prepared by low-temperature heating and is an aqueous solution, which is not convenient for transportation and storage. The magnesium phosphate gelling component uses active magnesium oxide as an alkali component, which has the defects of too fast coagulation time and inconvenient construction.

[0006] CN 113149597 A provides a potassium magnesium phosphate-based steel anticorrosion coating material and a preparation method thereof. Potassium dihydrogen phosphate is used as an acid component to prepare a potassium magnesium phosphate adhesive, which can achieve controllable coagulation time. However, the potassium magnesium phosphate hydrate generated by potassium salt is easily soluble in a neutral water environment, and the long-term water stability of the prepared coating hardened body is insufficient.

[0007] Application Contents

[0008] Technical issues solved:

[0009] The technical problems that need to be solved in this application are that the inorganic adhesive has harsh construction conditions, low-temperature film formation, slow curing speed, easy volume shrinkage and brittle coating during the curing process, phosphate anti-corrosion coatings must be baked at a relatively high temperature to achieve curing, are inconvenient for transportation and storage, have a too fast coagulation time and are inconvenient for construction, and the long-term water stability of the hardened coating is insufficient. Provide a magnesium ammonium phosphate-based steel substrate anti-corrosion coating and a preparation method thereof, which has excellent properties such as room temperature curing, fast hardening, high strength, strong adhesion to the steel substrate, good volume stability and water stability, and strong resistance to salt corrosion. In addition, the prepared hardened coating has good toughness and good compatibility with the steel substrate.

[0010] Technical solution:

[0011] A magnesium ammonium phosphate-based steel substrate anticorrosion coating, wherein the raw materials of the magnesium ammonium phosphate-based steel substrate anticorrosion coating are mixed by weight proportions of 82-90 parts of magnesium ammonium phosphate adhesive, 3-8 parts of retarder, 1-2 parts of defoamer, 5-8 parts of corrosion inhibition and enhancement components, and 0.5-1.5 parts of toughening components.

[0012] As a preferred technical solution of the present application: the magnesium ammonium phosphate adhesive is composed of 1 part of an acid component and 2.5-3.0 parts of an alkali component in a mass ratio.

[0013] As a preferred technical solution of the present application: the alkali component is composed of dead-burned oxide powder and metakaolin and / or sulphoaluminate cement.

[0014] As a preferred technical solution of the present application: the dead-burned magnesium oxide accounts for 80-90% of the alkali component, and the metakaolin and / or sulphoaluminate cement accounts for 10-20% of the alkali component.

[0015] As a preferred technical solution of the present application: the dead-burned magnesium oxide is obtained by calcining and grinding magnesite at a high temperature of 1300-1600°C, the MgO content in the dead-burned magnesium oxide is 88-92%, and the fineness after grinding is 200-300 mesh; the metakaolin is calcined at >800°C, and the fineness is 1000-1500 mesh; the fineness of sulphoaluminate cement is 400-800 mesh; the acid component is diammonium phosphate, industrial grade, NH4H2PO4 content ≥98%, and the crystal particle size is 60-150 mesh.

[0016] As a preferred technical solution of the present application: the retarder is borax and / or boric acid, in the form of crystalline powder, with a particle size in the range of 60 to 150 meshes, and is industrial grade.

[0017] As a preferred technical solution of the present application: the defoaming agent is a polyether-modified polysiloxane solid powder.

[0018] As a preferred technical solution of the present application: the corrosion inhibition and enhancement component is a composite of aluminum tripolyphosphate and its modified products and carboxymethyl chitosan, wherein the mass ratio of aluminum tripolyphosphate and its modified products to carboxymethyl chitosan is 1:0.3-0.8; aluminum tripolyphosphate and its modified products are of premium grade, with a fineness of 800-1250 meshes and a pH value of 5.5-7; carboxymethyl chitosan is food grade, with a carboxylation degree greater than 80% and a fineness of 800-1250 meshes.

[0019] As a preferred technical solution of the present application: the toughening component is basic magnesium sulfate whiskers, which are needle-shaped single crystals with a diameter D < 1.0 μm, an average length L of 10-60 μm, an aspect ratio L / D > 30, and a pH value of 9-9.5.

[0020] The present application also discloses a method for preparing a magnesium ammonium phosphate-based steel substrate anticorrosion coating, the steps of which are:

[0021] Step 1: Use a dry powder mixer to mix dead burnt magnesium oxide powder, metakaolin and / or sulphoaluminate cement, and retarder borax for 2 to 3 minutes and seal and package them as component A; use a dry powder mixer to mix the acid component ammonium dihydrogen phosphate, retarder boric acid, corrosion inhibition and strengthening component aluminum tripolyphosphate and its modified products, and carboxymethyl chitosan for 2 to 3 minutes and seal and package them as component B; mix the defoamer polyether modified polysiloxane solid powder and the toughening component basic magnesium sulfate whisker and seal and package them as component C;

[0022] Step 2: Mix the dry powders of components A and B obtained in the first step with water and stir for 2-3 minutes under natural environmental conditions of 5°C-30°C and 50%-80% RH, and finally add component C and stir for 3-5 minutes to obtain the magnesium ammonium phosphate-based steel substrate anticorrosive coating slurry; the amount of water added in the second step is based on the initial fluidity of the slurry reaching the specified requirements;

[0023] Step 3: The coating slurry is coated on the surface of the steel substrate once or twice by spraying or brushing to form an ammonium magnesium phosphate-based steel substrate anti-corrosion coating.

[0024] Technical principle:

[0025] Magnesium ammonium phosphate-based anti-corrosion coating for steel substrates has chemical ceramic properties, and the particles are connected by ionic bonds or covalent bonds. It has a dense structure and anti-penetration ability, which can prevent corrosive media from contacting the steel surface and corroding the steel (physical shielding). The phosphate in the magnesium ammonium phosphate main adhesive has a phosphating effect on the steel substrate, forming an insoluble film (phosphating film) on the steel surface, which further prevents the intrusion of corrosive ions and the occurrence of corrosion.

[0026] The retarding component in the magnesium ammonium phosphate-based anticorrosive coating for steel substrates controls the setting time and hydration rate of the fresh coating slurry by generating a borate protective film, dissolving to absorb heat and cool down, and adjusting the pH value. However, it inhibits the late reaction activity of the slurry, resulting in a low late strength of the hardened body. The addition of an appropriate amount of aluminum tripolyphosphate can not only serve as a corrosion inhibition component to improve the corrosion resistance of the coating, but also improve the late strength of the hardened body by stimulating the late hydration activity of the magnesium ammonium phosphate adhesive slurry; the addition of an appropriate amount of carboxymethyl chitosan can use its film-forming and adsorption effects to fill the capillary pores of the magnesium ammonium phosphate adhesive-based coating hardened body, thereby increasing the structural density of the coating hardened body and enhancing the physical protection effect, thereby improving the strength and corrosion resistance of the coating hardened body.

[0027] Beneficial effects:

[0028] The magnesium ammonium phosphate-based steel substrate anticorrosion coating and preparation method thereof described in the present application adopt the above technical scheme and have the following technical effects compared with the prior art:

[0029] 1. The magnesium ammonium phosphate-based anti-corrosion coating for steel substrates is a three-component solid powder, which is easy to store. The coating slurry preparation process is simple and can be constructed at room temperature. The slurry can ensure good workability within 20-50 minutes, and can be easily applied and repaired to steel facilities at the construction site. After the construction is completed, the coating can be cured autonomously in a normal atmospheric environment (5°C-30°C, 30%-80% RH) (the 3h flexural strength of the hardened coating of Examples 1-3 in Table 7 exceeds 9.0MPa, and the 3h compressive strength exceeds 35.0MPa), so as to avoid the need for special curing equipment and heating processes;

[0030] 2. The soluble phosphate in the coating slurry can combine with the iron element on the surface of the steel substrate to form a dense protective layer of iron phosphate compounds, which can not only protect the steel structure surface from rust, but also enhance the adhesion of the coating on the steel structure surface (the 3d bonding strength with the steel substrate is 5.0-6.0MPa). The main gelling hydration product, magnesium ammonium phosphate hexahydrate crystals or gel (struvite), has good stability in weak acid, neutral and weak alkaline corrosive environments (the bonding strength loss after immersion in weak acid, neutral and weak alkaline corrosive media for 90 days does not exceed 10%).

[0031] 3. The steel corrosion inhibition and enhancement component in the coating has both corrosion inhibition effect (comparing Table 8 with Example 1 and Reference 1, the initial polarization resistance is increased by 12.2%, the polarization resistance loss of Example 1 after 28 days of electrochemical experiment is 37.7%, and the polarization resistance loss of Reference 1 is 50.8%), and the reaction activity is enhanced (the hydration temperature peak is increased by 23.5℃, see Figure 1 The density of the hardened structure is improved by the adsorption effect (comparison between reference 1 and example 1) and the porosity of the hardened coating is reduced by 4.63% by comparison between comparative example 3 and comparative example 2), which has the dual effects of strengthening physical isolation and passive corrosion protection;

[0032] 4. The anti-corrosion coating uses basic magnesium sulfate whiskers as a toughness-enhancing component, which can effectively improve the flexibility of the coating (compare Example 3 and Example 1 in Table 7, the folding ratio of Example 1 is increased by 3.2%), ensuring that the hardened coating can deform in coordination with the substrate without cracking when the steel facility is subjected to elastic stress.

[0033] 5. Compared with the zinc-rich epoxy coating primer, one of the products with the best anti-corrosion performance currently, the basic anti-corrosion ability of the magnesium ammonium phosphate-based steel substrate anti-corrosion coating is appropriately improved (comparing Comparative Example 4 and Example 1 in Table 8, the initial polarization resistance is increased by 63.1%), and the anti-corrosion stability is greatly improved (comparing Comparative Example 4 and Example 1 in Table 8, the polarization resistance loss of Example 1 after 28 days of electrochemical experiment is 37.7%, and the polarization resistance loss of Reference 4 is 99.99%). BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is a hydration temperature curve of the magnesium ammonium phosphate adhesive-based coating slurry of the present application. DETAILED DESCRIPTION

[0035] In order to better understand the present invention, the content of the present invention is further explained in conjunction with the following examples, but the content of the present invention is not limited to the following examples.

[0036] Embodiment 1:

[0037] A magnesium ammonium phosphate-based steel substrate anti-corrosion coating, wherein the raw materials of the magnesium ammonium phosphate-based steel substrate anti-corrosion coating are mixed by weight proportions of 84 parts of magnesium ammonium phosphate adhesive, 7 parts of retarder, 1 part of defoamer, 7 parts of corrosion inhibition and enhancement components, and 1 part of toughening component.

[0038] A magnesium ammonium phosphate-based anticorrosive coating for a steel substrate, the coating being composed of a mixture of component A, component B and component C, wherein the components A, B and C are formulated as shown in Table 1.

[0039] Table 1 Magnesium ammonium phosphate adhesive-based steel structure anticorrosion coating formula

[0040]

[0041] In Table 1, the dead-burned magnesium oxide has a fineness of 220 mesh, the metakaolin has a fineness of 1000 mesh, the ammonium dihydrogen phosphate (crystal particle size is 60 mesh), and the fineness of aluminum tripolyphosphate (and its modified products) and carboxymethyl chitosan are both 1000 mesh.

[0042] Basic magnesium sulfate whiskers have high surface activity and hydrophilicity, good dispersibility in magnesium ammonium phosphate adhesive-based coating slurry, simple preparation and low cost, and can improve the brittleness of the coating hardened body and enhance its toughness and crack resistance.

[0043] A method for preparing a magnesium ammonium phosphate-based steel substrate anticorrosive coating comprises the following steps:

[0044] Step 1: Use a dry powder mixer to mix dead burnt magnesium oxide powder, metakaolin and / or sulphoaluminate cement, and retarder borax for 2 to 3 minutes and seal and package them as component A; use a dry powder mixer to mix the acid component ammonium dihydrogen phosphate, the corrosion inhibition and strengthening component aluminum tripolyphosphate and its modified product, and carboxymethyl chitosan for 2 to 3 minutes and seal and package them as component B; mix the defoamer polyether modified polysiloxane solid powder and the toughening component basic magnesium sulfate whisker and seal and package them as component C;

[0045] Step 2: Under the natural environment conditions of 5℃-30℃ and 50%-80%RH, mix and stir the dry powders of components A and B with an appropriate amount of water (based on the initial consistency of the coating slurry to meet the specified requirements) for 2-3 minutes to obtain the coating slurry, and finally add component C and mix and stir for 3-5 minutes to obtain the magnesium ammonium phosphate adhesive-based steel anticorrosion coating material slurry;

[0046] Step 3: The coating slurry is coated on the surface of the steel substrate once or twice by spraying or brushing to form an ammonium magnesium phosphate-based steel substrate anti-corrosion coating.

[0047] Table 4 shows the flexural and compressive strengths, flexural-compression ratio, and bonding strength with the steel substrate of the hardened coating.

[0048] Table 5 shows the polarization resistance obtained by analyzing the anode polarization curve, the charge transfer resistance obtained by electrochemical impedance spectroscopy (EIS) analysis, and the salt spray test results.

[0049] Embodiment 2:

[0050] A magnesium ammonium phosphate-based steel substrate anti-corrosion coating, wherein the raw materials of the magnesium ammonium phosphate-based steel substrate anti-corrosion coating are mixed by weight proportions of 88 parts of magnesium ammonium phosphate adhesive, 3 parts of retarder, 1 part of defoamer, 7 parts of corrosion inhibition and enhancement components, and 1 part of toughening component.

[0051] A magnesium ammonium phosphate-based anticorrosive coating for a steel substrate, the coating being composed of a mixture of component A, component B and component C, wherein the components A, B and C are formulated as shown in Table 2.

[0052] Table 2 Magnesium ammonium phosphate adhesive-based steel structure anticorrosion coating formula

[0053]

[0054] In Table 2, the dead-burned magnesium oxide has a fineness of 220 mesh, the metakaolin has a fineness of 1000 mesh, the ammonium dihydrogen phosphate (crystal particle size is 60 mesh), and the fineness of aluminum tripolyphosphate (and its modified products) and carboxymethyl chitosan are both 1000 mesh.

[0055] A method for preparing a magnesium ammonium phosphate-based steel substrate anticorrosive coating comprises the following steps:

[0056] Step 1: Use a dry powder mixer to stir and mix dead burnt magnesium oxide powder, metakaolin and / or sulphoaluminate cement for 2 to 3 minutes and seal and package them as component A; use a dry powder mixer to stir and mix the acid component ammonium dihydrogen phosphate, retarder boric acid, corrosion inhibition and strengthening component aluminum tripolyphosphate and its modified products, and carboxymethyl chitosan for 2 to 3 minutes and seal and package them as component B; use a dry powder mixer to mix the defoamer polyether modified polysiloxane solid powder and the toughening component basic magnesium sulfate whisker and seal and package them as component C;

[0057] Step 2: Under the natural environment conditions of 5℃-30℃ and 50%-80%RH, mix and stir the dry powders of components A and B with an appropriate amount of water (based on the initial consistency of the coating slurry to meet the specified requirements) for 2-3 minutes to obtain the coating slurry, and finally add component C and mix and stir for 3-5 minutes to obtain the magnesium ammonium phosphate adhesive-based steel anticorrosion coating material slurry;

[0058] Step 3: The coating slurry is coated on the surface of the steel substrate once or twice by spraying or brushing to form an ammonium magnesium phosphate-based steel substrate anti-corrosion coating.

[0059] Table 4 shows the flexural and compressive strengths, flexural-compression ratio, and bonding strength with the steel substrate of the hardened coating.

[0060] Table 5 shows the polarization resistance obtained by analyzing the anode polarization curve, the charge transfer resistance obtained by analyzing the electrochemical impedance spectroscopy (EIS), and the salt spray test results.

[0061] Embodiment 3:

[0062] A magnesium ammonium phosphate-based steel substrate anti-corrosion coating, wherein the raw materials of the magnesium ammonium phosphate-based steel substrate anti-corrosion coating are mixed by weight proportions of 84 parts of magnesium ammonium phosphate adhesive, 7 parts of retarder, 1 part of defoamer, 7 parts of corrosion inhibition and enhancement components, and 1 part of toughening component.

[0063] A magnesium ammonium phosphate-based anticorrosion coating for a steel substrate, the coating being composed of a mixture of component A, component B and component C, wherein the components A, B and C are formulated as shown in Table 3.

[0064] Table 3 Magnesium ammonium phosphate adhesive-based steel structure anticorrosion coating formula

[0065]

[0066] In Table 3, the fineness of dead-burned magnesium oxide is 280 mesh, the fineness of metakaolin is 1000 mesh, the particle size of ammonium dihydrogen phosphate is 150 mesh, the particle size of borax is 150 mesh, and the fineness of aluminum tripolyphosphate (and its modified products) and carboxymethyl chitosan are both 1000 mesh.

[0067] A method for preparing a magnesium ammonium phosphate-based steel substrate anticorrosive coating comprises the following steps:

[0068] Step 1: Use a dry powder mixer to mix dead burnt magnesium oxide powder, metakaolin and / or sulphoaluminate cement, and retarder borax for 2 to 3 minutes and seal and package them as component A; use a dry powder mixer to mix the acid component ammonium dihydrogen phosphate, the corrosion inhibition and strengthening component aluminum tripolyphosphate and its modified product, and carboxymethyl chitosan for 2 to 3 minutes and seal and package them as component B; mix the defoamer polyether modified polysiloxane solid powder and the toughening component basic magnesium sulfate whisker and seal and package them as component C;

[0069] Step 2: Under the natural environment conditions of 5℃-30℃ and 50%-80%RH, mix and stir the dry powders of components A and B with an appropriate amount of water (based on the initial consistency of the coating slurry to meet the specified requirements) for 2-3 minutes to obtain the coating slurry, and finally add component C and mix and stir for 3-5 minutes to obtain the magnesium ammonium phosphate adhesive-based steel anticorrosion coating material slurry;

[0070] Step 3: The coating slurry is coated on the surface of the steel substrate once or twice by spraying or brushing to form an ammonium magnesium phosphate-based steel substrate anti-corrosion coating.

[0071] Table 4 shows the flexural and compressive strengths, flexural-compression ratio, and bonding strength with the steel substrate of the hardened coating.

[0072] Table 5 shows the polarization resistance obtained by analyzing the anode polarization curve, the charge transfer resistance obtained by analyzing the electrochemical impedance spectroscopy (EIS), and the salt spray test results.

[0073] Comparative Example 1

[0074] In order to verify the effect of the dual doping of corrosion inhibition and reinforcement components and toughening components, a reference sample was added. Compared with Example 1, it can reflect the improvement effect of the dual doping of corrosion inhibition and reinforcement components and toughening components on the performance of the magnesium ammonium phosphate-based steel substrate anti-corrosion coating, wherein the acid-base ratio of the magnesium ammonium phosphate adhesive is consistent with that in Example 1.

[0075] A comparative sample of magnesium ammonium phosphate-based anti-corrosion coating for a steel substrate, wherein the raw materials of the magnesium ammonium phosphate-based anti-corrosion coating for a steel substrate are composed of 90 parts of magnesium ammonium phosphate adhesive, 8 parts of retarder, and 2 parts of defoamer in a weight ratio.

[0076] A comparative sample of an ammonium magnesium phosphate-based anticorrosive coating for a steel substrate, the coating being composed of a mixture of component A, component B and component C, wherein component A, component B and component C are formulated as shown in Table 4, respectively.

[0077] Table 4 Magnesium ammonium phosphate adhesive-based steel structure anticorrosion coating formula

[0078]

[0079] In Table 1, the dead-burned magnesium oxide is composed of 220 meshes, the metakaolin is composed of 1000 meshes, and diammonium phosphate (crystal particle size is 60 meshes).

[0080] A method for preparing a magnesium ammonium phosphate-based steel substrate anticorrosive coating comprises the following steps:

[0081] Step 1: Use a dry powder mixer to mix the dead burnt magnesium oxide powder, metakaolin, and retarder borax for 2 to 3 minutes and seal and package them as component A, seal and package the acid component ammonium dihydrogen phosphate as component B, and seal and package the defoaming agent polyether modified polysiloxane solid powder as component C;

[0082] Step 2: Under the natural environment conditions of 5℃-30℃, 50%-80%RH, mix and stir the dry powder of components A and B with an appropriate amount of water (based on the initial consistency of the coating slurry to meet the specified requirements) for 2-3 minutes to obtain the coating slurry, and finally add component C and mix and stir for 3-5 minutes to obtain the magnesium ammonium phosphate adhesive-based steel anticorrosive coating material slurry comparison sample;

[0083] Step 3: The coating slurry is coated on the surface of the steel substrate once or twice by spraying or brushing to form an ammonium magnesium phosphate-based steel substrate anti-corrosion coating.

[0084] Comparative Example 2:

[0085] In order to verify the effect of the single corrosion inhibition and enhancement component aluminum tripolyphosphate, a reference sample was added. Compared with comparative example 1, it can reflect the effect of aluminum tripolyphosphate, wherein the acid-base ratio of the magnesium ammonium phosphate adhesive is consistent with that in example 1.

[0086] A comparative sample of magnesium ammonium phosphate-based anti-corrosion coating for a steel substrate, wherein the raw materials of the magnesium ammonium phosphate-based anti-corrosion coating for a steel substrate are composed of 86 parts of magnesium ammonium phosphate adhesive, 7 parts of retarder, 5.5 parts of corrosion inhibition and enhancement component and 1.5 parts of defoamer in proportion by mass.

[0087] A comparative sample of an ammonium magnesium phosphate-based anticorrosive coating for a steel substrate, the coating being composed of a mixture of component A, component B and component C, wherein component A, component B and component C are formulated as shown in Table 5, respectively.

[0088] Table 5 Magnesium ammonium phosphate adhesive-based steel structure anticorrosion coating formula

[0089]

[0090] A method for preparing a magnesium ammonium phosphate-based steel substrate anticorrosive coating comprises the following steps:

[0091] Step 1: Use a dry powder mixer to mix dead burnt magnesium oxide powder, metakaolin and retarder borax for 2 to 3 minutes and seal and package them as component A; use a dry powder mixer to mix the acid component ammonium dihydrogen phosphate, the corrosion inhibition and enhancement component aluminum tripolyphosphate and its modified product for 2 to 3 minutes and seal and package them as component B; and seal and package the defoaming agent polyether modified polysiloxane solid powder as component C;

[0092] Step 2: Under the natural environment conditions of 5℃-30℃ and 50%-80%RH, mix and stir the dry powders of components A and B with an appropriate amount of water (based on the initial consistency of the coating slurry to meet the specified requirements) for 2-3 minutes to obtain the coating slurry, and finally add component C and mix and stir for 3-5 minutes to obtain the magnesium ammonium phosphate adhesive-based steel anticorrosion coating material slurry;

[0093] Step 3: The coating slurry is coated on the surface of the steel substrate once or twice by spraying or brushing to form an ammonium magnesium phosphate-based steel substrate anti-corrosion coating.

[0094] Table 4 shows the flexural and compressive strengths, flexural-compression ratio, and bonding strength with the steel substrate of the hardened coating.

[0095] Table 5 shows the polarization resistance obtained by analyzing the anode polarization curve, the charge transfer resistance obtained by analyzing the electrochemical impedance spectroscopy (EIS), and the salt spray test results.

[0096] Comparative Example 3:

[0097] In order to verify the effect of the corrosion inhibition and strengthening components aluminum tripolyphosphate and carboxymethyl chitosan, the reference sample was added. Compared with Example 2, the effect of carboxymethyl chitosan can be reflected. Comparing Example 1 with this example, the effect of the toughening component can be reflected. The acid-base ratio of the magnesium ammonium phosphate adhesive is consistent with that of Example 1.

[0098] A comparative sample of magnesium ammonium phosphate-based anti-corrosion coating for a steel substrate, wherein the raw materials of the magnesium ammonium phosphate-based anti-corrosion coating for a steel substrate are composed of 86 parts of magnesium ammonium phosphate adhesive, 7 parts of retarder, 5.5 parts of corrosion inhibition and enhancement component and 1.5 parts of defoamer in proportion by mass.

[0099] A comparative sample of an ammonium magnesium phosphate-based anticorrosive coating for a steel substrate, the coating being composed of a mixture of component A, component B and component C, wherein component A, component B and component C are formulated as shown in Table 6, respectively.

[0100] Table 6 Magnesium ammonium phosphate adhesive-based steel structure anticorrosion coating formula

[0101]

[0102]

[0103] A method for preparing a magnesium ammonium phosphate-based steel substrate anticorrosive coating comprises the following steps:

[0104] Step 1: Use a dry powder mixer to mix dead burnt magnesium oxide powder, metakaolin and retarder borax for 2 to 3 minutes and seal and package them as component A; use a dry powder mixer to mix the acid component ammonium dihydrogen phosphate, the corrosion inhibition and enhancement component aluminum tripolyphosphate and its modified product, and carboxymethyl chitosan for 2 to 3 minutes and seal and package them as component B; and seal and package the defoaming agent polyether modified polysiloxane solid powder as component C;

[0105] Step 2: Under the natural environment conditions of 5℃-30℃ and 50%-80%RH, mix and stir the dry powders of components A and B with an appropriate amount of water (based on the initial consistency of the coating slurry to meet the specified requirements) for 2-3 minutes to obtain the coating slurry, and finally add component C and mix and stir for 3-5 minutes to obtain the magnesium ammonium phosphate adhesive-based steel anticorrosion coating material slurry;

[0106] Step 3: The coating slurry is coated on the surface of the steel substrate once or twice by spraying or brushing to form an ammonium magnesium phosphate-based steel substrate anti-corrosion coating.

[0107] Table 4 shows the flexural and compressive strengths, flexural-compression ratio, and bonding strength with the steel substrate of the hardened coating.

[0108] Table 5 shows the polarization resistance obtained by analyzing the anode polarization curve, the charge transfer resistance obtained by analyzing the electrochemical impedance spectroscopy (EIS), and the salt spray test results.

[0109] Application performance testing

[0110] The anti-corrosion coatings prepared in the above Examples 1-3 and Comparative Examples 1-3 were respectively tested for flexural strength, compressive strength (3h, 3d and 28d) and porosity, and the bonding strength between the hardened coating and the steel substrate was tested (3d). The results obtained are shown in Table 7.

[0111] Referring to GB / T 17671-2021 "Test Method for Cement Mortar Strength", 40mm×40mm×160mm prism specimens were used to test the flexural strength and compressive strength of the hardened coating at different ages. The coating bonding strength test was based on the GB / T5210-2006 standard. After the end face of the cylindrical sample with a diameter of 25mm was coated with the coating, it was cured at room temperature (25℃) for 3d; a universal material testing machine was used to stretch it at a rate of 1mm / min until the bonding surface broke, and the bonding strength between the coating and the substrate was calculated based on the fracture load. The porosity of the hardened coating was analyzed by low-field nuclear magnetic resonance testing. The LF1HNMR spectrometer produced by Limecho was used, with a fixed magnetic field of 0.5T and a corresponding proton resonance frequency of 2MHz. The temperature of the magnet and probe assembly was kept constant at 32±0.01℃. The stirred coating slurry was poured into a 50ml plastic sealed jar for curing for 48h, and the internal pore distribution and porosity of the coating sample were tested.

[0112] Table 7 Mechanical properties and porosity of hardened coating

[0113]

[0114]

[0115] *Comparative Example 4 is a 250 μm thick zinc-rich epoxy coating primer;

[0116] As shown in Table 4, the magnesium ammonium phosphate adhesive-based steel anticorrosive coatings prepared in Examples 1-3 of the present invention have a 28d strength, especially a fold-to-compression ratio, which is significantly higher than that of Comparative Example 3, verifying the toughening effect of basic magnesium sulfate whiskers. Comparative Example 2 is compared with Comparative Example 1, and the folding and compressive strengths and the bonding strength with the steel substrate are significantly improved, indicating that aluminum tripolyphosphate has a good reinforcing effect. Comparative Example 3 is compared with Comparative Example 2, and the folding and compressive strengths and the bonding strength with the steel substrate are significantly improved, indicating that the composite reinforcement component has a better reinforcing effect than single-doped aluminum tripolyphosphate, and the porosity of the coating hardened body of Comparative Example 3 and Comparative Example 2 is significantly reduced, indicating that aluminum tripolyphosphate and carboxymethyl chitosan are composited and have a good dense filling effect.

[0117] Potentiodynamic polarization curve and electrochemical impedance spectroscopy (EIS) tests used a steel substrate with a size of 15mm×15mm×2mm, on which the thickness of the magnesium ammonium phosphate adhesive-based steel anti-corrosion coating was 800μm. The electrochemical test used a three-electrode system: the reference electrode was a saturated calomel electrode (SCE), the auxiliary electrode was a platinum sheet, the electrolyte solution was a 3.5% NaCl solution, and the working electrodes were the coating samples immersed for different times; the experimental parameters used in the polarization curve test were: the potential scanning range was ±250mV relative to the open circuit potential (OPC), the potential scanning rate was 2mV / s, and the test data was analyzed and processed using Cview; the experimental parameters used in the electrochemical impedance spectroscopy (EIS) were: the AC disturbance signal was 15mV, the frequency range was 10 -2 Hz to 10 5 Hz, and Zsimpwin software was used to fit the equivalent circuit; all tests were performed after the open circuit potential was stabilized, and the ambient temperature was 25°C during the test.

[0118] Salt spray corrosion refers to the national standard ISO9227-2006 "Artificial atmosphere corrosion test salt spray test". The steel plate size used in the test is 150mm×70mm×2mm, the coating thickness is 800μm, the mass concentration of NaCl solution is 5.0±0.5%, and the continuous spraying is 1440h.

[0119] Table 8 Electrochemical test and salt spray test results of anti-corrosion coating material specimens

[0120]

[0121]

[0122] *Comparative Example 4 is a 250 μm thick zinc-rich epoxy coating primer;

[0123] As can be seen from Table 5, the initial values ​​of polarization resistance (Rp) and charge transfer resistance (Rct) of the polarization curve of magnesium ammonium phosphate adhesive-based steel anticorrosion coatings prepared in Examples 1-3 of the present invention are slightly higher than those of Comparative Example 4 (zinc-rich epoxy coating primer). After the coating samples were immersed in a 3.5% NaCl solution for 28 days, electrochemical tests were continued. The Rp and Rct obtained from the analysis of the samples of Examples 1-3 were 2 orders of magnitude higher than those of Reference 4, indicating that the anticorrosion stability of the samples of Examples 1-3 was much higher than that of Comparative Example 4. The results of the salt spray test also showed that the anticorrosion ability of Examples 1-3 in both stress-free and stress-containing states was significantly better than that of Comparative Example 4. Comparing Comparative Example 1 with Comparative Example 2, the initial Rp and Rct of the coating sample of Comparative Example 2 and the Rp and Rct of the sample immersed in the salt solution for 28 days were significantly higher than those of Comparative Example 1, confirming the corrosion inhibition effect of aluminum tripolyphosphate. Comparing Comparative Example 3 with Comparative Example 2, the initial Rp and Rct of the coating sample of Comparative Example 3 and the Rp and Rct of the coating sample after 28 days of immersion in salt solution are slightly higher than those of Comparative Example 2, which confirms that the corrosion inhibition effect of aluminum tripolyphosphate and carboxymethyl chitosan can be further enhanced. Comparing Examples 1-3 with Comparative Example 3, the initial Rp and Rct of the samples of Examples 1-3 and the Rp and Rct of the coating sample after 28 days of immersion in salt solution are higher than those of the samples of Comparative Example 3, indicating that the addition of magnesium sulfate whiskers can improve the corrosion resistance of the coating samples. The salt spray test results of the samples subjected to 25MPa stress show that magnesium sulfate whiskers have a good toughening effect and can improve the synergistic force bearing capacity of the coating and the steel substrate.

[0124] Figure 1 It is the hydration temperature curve of comparative example 1, comparative example 2 and examples 1-3. It can be seen from the figure that due to the endothermic dissolution of the retarder borax and the acid component composite phosphate, the system temperature drops rapidly, and the lowest temperature is nearly 10°C lower than the room temperature. Then the temperature of the slurry gradually rises, but the temperature of the slurry does not exceed 35°C (initial setting temperature) within 20 minutes, indicating that the initial setting time of the coating slurry is greater than 20 minutes. Because the retarder borax (or boric acid) inhibits the acid-base reaction activity of the magnesium ammonium phosphate adhesive, the highest hydration temperature of comparative example 1 is only 66.7°C, resulting in low early and late strengths of the coating hardened body (see Table 7). In comparative example 2, the hydration activity of the coating slurry doped with aluminum tripolyphosphate reinforcing component is stimulated, and the highest hydration temperature of the slurry is increased to 89.6°C, which ultimately significantly improves the early and late strengths of the coating hardened body (Table 7). In Example 1, aluminum tripolyphosphate and carboxymethyl chitosan were doped as reinforcing components, and the hydration activity of the coating slurry was further stimulated, so that the maximum hydration temperature of the slurry was increased to 90.2°C, and the early and late strengths of the hardened coating were improved compared with those of Comparative Example 2 (Table 7).

[0125] The above descriptions are only some embodiments of the present invention. It should be pointed out that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A magnesium ammonium phosphate-based anticorrosion coating for steel substrate, characterized in that: The raw materials of the magnesium ammonium phosphate-based steel substrate anticorrosive coating are mixed by weight proportion of 82-90 parts of magnesium ammonium phosphate adhesive, 5-8 parts of retarder, 1-2 parts of defoamer, 5-8 parts of corrosion inhibition and enhancement component and 0.5-1.5 parts of toughening component; the magnesium ammonium phosphate adhesive is composed of 1 part of acid component and 2.5-3.0 parts of alkali component by weight proportion; the alkali component is composed of dead burnt magnesium oxide powder and metakaolin; the dead burnt magnesium oxide powder is obtained by calcining and grinding magnesite at a high temperature of 1300-1600°C, the MgO content in the dead burnt magnesium oxide powder is 88-92%, and the fineness after grinding is 200-300 mesh; metakaolin is calcined at >800°C and has a fineness of 1000-1500 mesh; the corrosion inhibition and enhancement component is a composite of aluminum tripolyphosphate and its modified products and carboxymethyl chitosan, wherein the mass ratio of aluminum tripolyphosphate and its modified products to carboxymethyl chitosan is 1:0.3-0.8; aluminum tripolyphosphate and its modified products are of superior grade, with a fineness of 800-1250 mesh and a pH value of 5.5-7; carboxymethyl chitosan is of food grade, with a carboxylation degree greater than 80% and a fineness of 800-1250 mesh; the retarder is borax and / or boric acid, in the form of crystalline powder, with a particle size in the range of 60-150 mesh, and is of industrial grade.

2. The magnesium ammonium phosphate-based steel substrate anticorrosion coating according to claim 1, characterized in that: The dead-burned magnesium oxide powder accounts for 80-90% of the alkali component, and the metakaolin accounts for 10-20% of the alkali component.

3. The magnesium ammonium phosphate-based anticorrosion coating for steel substrate according to claim 1, characterized in that: The acid component is ammonium dihydrogen phosphate, industrial grade, NH4H2PO4 content ≥ 98%, and crystal particle size of 60-150 meshes.

4. The magnesium ammonium phosphate-based anticorrosion coating for steel substrate according to claim 1, characterized in that: The defoamer is polyether-modified polysiloxane solid powder.

5. The magnesium ammonium phosphate-based anticorrosion coating for steel substrate according to claim 1, characterized in that: The toughening component is basic magnesium sulfate whisker, which is a needle-shaped single crystal with a diameter D less than 1.0 μm, an average length L of 10-60 μm, an aspect ratio L / D greater than 30, and a pH value of 9-9.

5.

6. A method for preparing the magnesium ammonium phosphate-based anticorrosive coating for steel substrates according to any one of claims 1 to 5, characterized in that: The steps are: Step 1: Use a dry powder mixer to mix dead burnt magnesium oxide powder, metakaolin, and retarder borax for 2 to 3 minutes and seal and package them as component A; use a dry powder mixer to mix the acid component ammonium dihydrogen phosphate, retarder boric acid, corrosion inhibition and strengthening component aluminum tripolyphosphate and its modified products, and carboxymethyl chitosan for 2 to 3 minutes and seal and package them as component B; mix the defoamer polyether modified polysiloxane solid powder and the toughening component basic magnesium sulfate whisker and seal and package them as component C; Step 2: Mix the dry powders of components A and B obtained in the first step with water and stir for 2 to 3 minutes under natural environmental conditions of 5°C to 30°C and 50% to 80% RH, and finally add component C and stir for 3 to 5 minutes to obtain the magnesium ammonium phosphate-based steel substrate anticorrosive coating slurry; the amount of water added is based on the initial fluidity of the slurry reaching the specified requirements; Step 3: The coating slurry is applied once or twice to the surface of the steel substrate by spraying or brushing to form an ammonium magnesium phosphate-based steel substrate anti-corrosion coating.