A positive electrode material and preparation method thereof and sodium ion battery
By double-layer coating of Prussian blue positive electrode material, using tanninic acid polymer and other materials to form a hydrophobic layer, the problem of Prussian blue is solved, the storage stability and electrochemical performance are improved, and the environment is ensured in high humidity. Excellent performance.
Patent Information
- Application Number
- CN202311041962.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-17
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-08-17
AI Technical Summary
Prussian blue positive electrode material is prone to moisture absorption in air environments, resulting in poor processing performance, poor sodium storage performance and battery safety. The existing high-temperature heat treatment methods cannot completely suppress hygroscopy.
The Prussian blue matrix is coated using a double-layer coating technology. The first coating layer is composed of a polymer of tannin, and the second coating layer includes hexadecimal, octamine, octadecimal phosphate, N- Materials such as phenylbistrifluoromethanesulfonate and perfluoride form a hydrophobic layer and reduce hygroscopicity.
It effectively improves the storage stability and electrochemical performance of Prussian blue cathode materials in the air, ensuring that excellent circulation and rate performance can be maintained under high humidity environments.
Smart Images

Figure CN116864656B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a positive electrode material and a preparation method thereof, and a sodium ion battery. Background Art
[0002] Prussian blue (PB) is an important cathode material for sodium ion batteries. x M a M' b (CN)6·zH2O, where 0 <x<2,0<a<1,0<b<1,z> 0, M and M' represent transition metals. Prussian blue cathode material has the advantages of high theoretical capacity, large interstitial position, adjustable chemical composition, good structural stability, etc., showing very excellent electrochemical performance; at the same time, this material has the advantages of being cheap, non-toxic, simple to prepare, and low in energy consumption, and is a cathode material with great commercial application prospects in sodium ion battery research.
[0003] There are still some problems to be solved for Prussian blue as a positive electrode material for sodium-ion batteries. Prussian blue is usually prepared by a simple chemical precipitation method, which leads to vacancy defects and crystal water in the material structure, where the crystal water consists of adsorbed water, interstitial water and coordinated water. The crystal water in the structure will have serious negative effects on electrode materials and electrolytes, such as affecting sodium ion migration, side reactions with electrolytes, and gas production affecting battery safety. Although most of the adsorbed water and interstitial water in the material can be removed by high-temperature heat treatment, the dehydrated Prussian blue will absorb water quickly when exposed to air and has strong hygroscopicity. In the manufacturing process of sodium-ion batteries, Prussian blue has to go through pulping, coating, rolling, slicing, winding / stacking, liquid injection, formation, packaging and other processes. In these processes, coating, rolling, slicing, winding / stacking are mostly exposed to the air environment. Due to the hygroscopic properties of Prussian blue, the processing performance of the pole piece is poor, and the adsorbed water will seriously affect its sodium storage performance and battery safety.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] The first object of the present invention is to provide a positive electrode material that can suppress the hygroscopicity of the material without affecting the electrochemical performance of Prussian blue, thereby effectively improving the storage stability and electrochemical performance of the positive electrode material in the air.
[0006] The second object of the present invention is to provide a method for preparing the above-mentioned positive electrode material, which has simple steps and is suitable for large-scale industrial production.
[0007] The third object of the present invention is to provide a sodium ion battery, comprising the above-mentioned positive electrode material, which has excellent electrochemical properties.
[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0009] The present invention provides a positive electrode material, comprising a Prussian blue matrix, and a first coating layer and a second coating layer sequentially coated on the surface of the Prussian blue matrix;
[0010] The material forming the first coating layer includes a polymer of tannic acid;
[0011] The material forming the second coating layer includes at least one of hexadecylamine, octadecylamine, octadecyl phosphate, N-phenylbis(trifluoromethanesulfonic acid)imide, 1H,1H,2H,2H-perfluorodecyltriethoxysilane and 1H,1H,2H,2H-perfluorodecylthiol.
[0012] The present invention also provides a method for preparing the positive electrode material as described above, comprising the following steps:
[0013] Mixing tannic acid, formaldehyde, ammonium ions, a first solvent and water to obtain a precursor solution containing tannic acid;
[0014] The Prussian blue matrix and the precursor solution containing tannic acid undergo a first reaction to obtain PB@TA;
[0015] The PB@TA, the material forming the second coating layer and the second solvent undergo a second reaction to obtain the positive electrode material.
[0016] The present invention also provides a sodium ion battery, comprising the positive electrode material as described above.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] 1. The cathode material provided by the present invention effectively solves the problem of easy moisture absorption of the Prussian blue cathode material by double-coating the Prussian blue matrix without affecting the electrochemical performance, and effectively improves the storage property and electrochemical performance of the cathode material in the air.
[0019] 2. The method for preparing the positive electrode material provided by the present invention can evenly coat the surface of the Prussian blue substrate with two coating layers, effectively suppressing the hygroscopicity of the material, and the steps are simple.
[0020] 3. The positive electrode material of the present invention is used in a sodium ion battery, which not only ensures that the sodium ion battery has excellent cycle performance and rate performance, but also improves the storage performance in a high humidity environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0022] Figure 1 2. XRD diagrams of PB and PB@TA@ODA of Example 1 of the present invention.
[0023] Figure 2 This is the SEM image of PB@TA@ODA of Example 1 of the present invention.
[0024] Figure 3 TG curves of PB and PB-7D of Example 1 of the present invention.
[0025] Figure 4 TG curves of PB@TA@ODA and PB@TA@ODA-7D of Example 1 of the present invention.
[0026] Figure 5 This is an optical photograph of the wetting angle of the positive electrode sheet made using the PB of Example 1 of the present invention.
[0027] Figure 6 This is an optical photograph of the wetting angle of the positive electrode sheet prepared using PB@TA@ODA in Example 1 of the present invention.
[0028] Figure 7 The charge and discharge curves of the sodium ion battery prepared by using the PB and PB@TA@ODA of Example 1 respectively.
[0029] Figure 8 This is the cycle curve of the sodium ion battery prepared using the PB and PB@TA@ODA of Example 1 of the present invention.
[0030] Fig. 9 The charge and discharge curves of the sodium ion battery prepared by using PB-7D and PB@TA@ODA-7D in Example 1 of the present invention.
[0031] Fig.10 The cycle curves of the sodium ion battery prepared using PB-7D and PB@TA@ODA-7D in Example 1 of the present invention. DETAILED DESCRIPTION
[0032] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0033] In a first aspect, some embodiments of the present invention provide a positive electrode material, including a Prussian blue matrix, and a first coating layer and a second coating layer sequentially coated on the surface of the Prussian blue matrix;
[0034] The material forming the first coating layer includes a polymer of tannic acid;
[0035] The material forming the second coating layer includes at least one of hexadecylamine, octadecylamine, octadecyl phosphate, N-phenylbistrifluoromethanesulfonic acid imide, 1H,1H,2H,2H-perfluorodecyltriethoxysilane and 1H,1H,2H,2H-perfluorodecylthiol.
[0036] In the positive electrode material of the present invention, the polymer of tannic acid is uniformly and completely coated on the surface of the Prussian blue matrix to form a first coating layer, namely the tannic acid polymer layer; the second coating layer is coated on the surface of the first coating layer and is connected to the first coating layer through a chemical bond.
[0037] The positive electrode material of the present invention changes the surface of the Prussian blue substrate from hydrophilic to hydrophobic by double-coating the surface of the Prussian blue substrate. Studies have shown that the positive electrode material provided by the present invention loses less weight at 150-250° C. after being placed under normal temperature, normal pressure and high humidity conditions for 7 days. Therefore, the positive electrode material provided by the present invention has good hygroscopicity suppression under normal temperature, normal pressure and high humidity conditions, and effectively solves the problem that the Prussian blue positive electrode material is easy to absorb moisture without affecting the electrochemical performance, so that the positive electrode material has good storage performance in the air and excellent electrochemical performance.
[0038] In the positive electrode material of the present invention, the Prussian blue matrix serves as an active substance, the first coating layer provides bonding groups for the second coating layer, and the second coating layer forms a hydrophobic coating layer; through the mutual cooperation of the three, the Prussian blue positive electrode material has excellent electrochemical performance and good environmental storage properties.
[0039] In a preferred embodiment, the chemical formula of the Prussian blue matrix is Na x M a M'b (CN)6·zH2O; wherein M and M' are each independently selected from at least one of Ni, Cu, Fe, Mn, Co and Zn, 0 <x<2,0<a<1,0<b<1,z> 0. M and M' may be the same or different.
[0040] In a preferred embodiment, the Prussian blue matrix comprises Na x Fe a [Fe b (CN)6]·zH2O、Na x Mn a [Fe b (CN)6]·zH2O、Na x Ni a [Fe b (CN)6]·zH2O and Na x Co a [Fe b (CN)6]·zH2O.
[0041] In a preferred embodiment, the particle size of the positive electrode material is 200-300 nm; typically but not limiting, for example, the particle size of the positive electrode material is 200 nm, 220 nm, 240 nm, 260 nm, 280 nm, 300 nm or a range consisting of any two thereof.
[0042] In a preferred embodiment, the thickness of the first coating layer is 3-4 nm; typically but not limiting, for example, the thickness of the first coating layer may be 3 nm, 3.5 nm, 4 nm, or a range of any two thereof.
[0043] In a preferred embodiment, the thickness of the second coating layer is 1-2 nm; typically but not limiting, for example, the thickness of the second coating layer may be 1 nm, 1.5 nm, 2 nm, or a range of any two thereof.
[0044] In the positive electrode material of the present invention, if the thickness of the first coating layer is too high, it will affect the interfacial transport of sodium ions, and if it is too low, a complete coating layer cannot be formed; if the thickness of the second coating layer is too high, it will affect the interfacial transport of sodium ions, and if it is too low, it will not have good hydrophobicity.
[0045] In a second aspect, some embodiments of the present invention further provide a method for preparing the above-mentioned positive electrode material, comprising the following steps:
[0046] Mixing tannic acid, formaldehyde, ammonium ions, a first solvent and water to obtain a precursor solution containing tannic acid;
[0047] The Prussian blue matrix (PB) and the precursor solution containing tannic acid undergo a first reaction to obtain PB@TA;
[0048] PB@TA, the material forming the second coating layer and the second solvent undergo a second reaction to obtain a positive electrode material.
[0049] The present invention conducts a first reaction between a precursor solution of tannic acid and a Prussian blue matrix, wherein tannic acid, formaldehyde and ammonium ions undergo a Mannich reaction, condense to form a tannic acid polymer, and form a uniform tannic acid polymer layer on the surface of the Prussian blue matrix to obtain a Prussian blue matrix coated with the tannic acid polymer (PB@TA); then, a hydrophobic material is used for coating, for example, octadecylamine undergoes a Michael addition reaction or a Schiff base reaction with a hydroxyl group or a carbonyl group in the tannic acid polymer to form a second coating layer on the surface of the PB@TA, thereby obtaining a positive electrode material (PB@TA@ODA) with a double-layer coating structure.
[0050] In a preferred embodiment, the temperature of the first reaction and the second reaction is each independently 25 to 80°C; the time of the first reaction and the second reaction is each independently 1 to 72 h; typically but not limitatively, for example, the temperature of the first reaction and the second reaction can each independently be 25°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C or a range consisting of any two thereof; the time of the first reaction and the second reaction can each independently be 1 h, 10 h, 20 h, 30 h, 40 h, 50 h, 60 h, 70 h or a range consisting of any two thereof.
[0051] In a preferred embodiment, after the first reaction, the process further includes a first washing and a first drying; after the second reaction, the process further includes a second washing and a second drying; preferably, the drying temperature is 50-200°C.
[0052] In a preferred embodiment, the molar ratio of tannic acid to formaldehyde is (0.022-0.024):1; preferably 0.023:1.
[0053] In a preferred embodiment, the substance providing ammonium ions includes ammonia water.
[0054] In a preferred embodiment, the concentration of ammonia water is 20-30 wt%, and the dosage ratio of ammonia water and tannic acid is 1 mL: 0.1-1 mmol; typically but not limiting, for example, the dosage ratio of ammonia water and tannic acid is 1 mL: 0.1 mmol, 1 mL: 0.3 mmol, 1 mL: 0.5 mmol, 1 mL: 0.7 mmol, 1 mL: 1 mmol or a range of any two thereof.
[0055] In a preferred embodiment, a method for preparing a precursor solution containing tannic acid comprises: mixing a tannic acid aqueous solution, a formaldehyde aqueous solution, ammonia water, a first solvent and water to obtain a precursor solution containing tannic acid; preferably, the concentration of the tannic acid aqueous solution is 0.01-0.02 mol / L, the concentration of the formaldehyde aqueous solution is 2-5 wt%, and the concentration of the ammonia water is 20-30 wt%; more preferably, the volume ratio of ammonia water to the tannic acid aqueous solution is 1:(15-25), preferably 1:20.
[0056] In a preferred embodiment, the pH value of the first reaction system is 6-7.
[0057] Tannic acid, formaldehyde and ammonium radicals undergo a Mannich reaction to condense into a polymer of tannic acid. The above amount of ammonia water can provide enough NH4 + , speeding up the reaction rate.
[0058] In a preferred embodiment, the mass ratio of Prussian blue matrix to tannic acid is 1:(0.05-2); typically but not limiting, for example, the mass ratio of Prussian blue matrix to tannic acid is 1:0.05, 1:0.08, 1:0.1, 1:0.2, 1:0.4, 1:0.6, 1:0.8, 1:1, 1:1.2, 1:1.4, 1:1.6, 1:1.8, 1:2 or a range of values of any two components therein; preferably, the mass ratio of Prussian blue matrix to tannic acid is 1:(0.15-0.2).
[0059] In a preferred embodiment, the mass ratio of PB@TA to the material forming the second coating layer is 1:(0.1-5); typically but not limitatively, for example, the mass ratio of PB@TA to the material forming the second coating layer can be 1:0.1, 1:0.5, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5 or a range of any two thereof; preferably, the mass ratio of PB@TA to the material of the second coating layer is 1:(0.8-1.2).
[0060] In a preferred embodiment, the first solvent comprises ethanol.
[0061] In a preferred embodiment, the mass ratio of tannic acid to the first solvent is 1:(45-50).
[0062] In a preferred embodiment, the volume ratio of the first solvent to water is (0.01-1):1.
[0063] In a preferred embodiment, the second solvent includes at least one of methanol, ethanol, ethylene glycol, acetone and tetrahydrofuran.
[0064] In a preferred embodiment, the mass ratio of the material of the second coating layer to the second solvent is 1:
[0065] (50~55).
[0066] In a preferred embodiment, the preparation method of the Prussian blue matrix includes a liquid phase method or a solid phase method.
[0067] In a preferred embodiment, the method for preparing the Prussian blue matrix comprises the following steps:
[0068] The Prussian blue matrix is obtained by reacting an aqueous solution of Na4Fe(CN)6 with an aqueous solution of a soluble metal salt;
[0069] The soluble metal salt includes sodium citrate and at least one of Ni salt, Cu salt, Fe salt, Mn salt, Co salt and Zn salt.
[0070] In a preferred embodiment, the method for preparing the Prussian blue matrix comprises the following steps:
[0071] Na4Fe(CN)6 and metal salt are ball-milled to obtain a Prussian blue matrix; wherein the metal salt includes at least one of Ni salt, Cu salt, Fe salt, Mn salt, Co salt and Zn salt.
[0072] In a third aspect, some embodiments of the present invention also provide a sodium ion battery comprising the above-mentioned positive electrode material.
[0073] The positive electrode material of the present invention is used in a sodium ion battery, which improves the storage performance under normal temperature, normal pressure and high humidity while ensuring that the sodium ion battery has excellent cycle performance and rate performance.
[0074] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0075] Example 1
[0076] The method for preparing the positive electrode material provided in this embodiment comprises the following steps:
[0077] S1. Take 4 mmol of Na4Fe(CN)6·10H2O and dissolve it in 200 mL of deionized water to form solution A; take 6 mmol of FeSO4·7H2O and 15 g of sodium citrate and dissolve them in 200 mL of deionized water to form solution B;
[0078] Solution A was added to solution B, and then allowed to stand at room temperature (25°C) for 6 hours, solid-liquid separation was performed to obtain a filter cake, which was washed three times by centrifugation with deionized water and anhydrous ethanol, respectively, and dried in a forced air drying oven at 80°C for 12 hours to obtain Prussian blue matrix (PB) Na 1.54 Fe[Fe(CN)6]·0.96H2O.
[0079] S2, adding 2 mL of 0.015 M tannic acid aqueous solution, 1 mL of formaldehyde aqueous solution (3.7 wt %), 0.1 mL of ammonia water (25 wt %) and 3 mL of ethanol to 13 mL of deionized water, and mixing thoroughly to obtain a tannic acid precursor solution;
[0080] 0.3 g of Na 1.54 Fe[Fe(CN)6]·0.96H2O was added to the tannic acid precursor solution, stirred continuously for 24 h at room temperature (25°C), filtered, and vacuum dried at 80°C to obtain PB@TA.
[0081] S3, adding 0.3 g of octadecylamine into 20 mL of ethanol and fully dissolving it to obtain an octadecylamine precursor solution;
[0082] 0.3 g of PB@TA was added to the octadecylamine precursor solution, stirred continuously for 24 h at room temperature (25°C), filtered, and vacuum dried at 80°C to obtain the positive electrode material (PB@TA@ODA).
[0083] Example 2
[0084] The method for preparing the positive electrode material provided in this embodiment comprises the following steps:
[0085] S1. Under an inert atmosphere, 5 mmol of MnCl2·4H2O and 5 mmol of Na4Fe(CN)6·10H2O were added to an agate ball mill with a ball-to-material ratio of 1:20. After ball milling at a rate of 300 r / min for 12 h, a mixed material was obtained. The mixed material was first washed with anhydrous ethanol and centrifuged three times, then washed with deionized water and centrifuged three times, and then dried in a vacuum oven at 80°C for 12 h to obtain Prussian blue matrix (PB) Na 1.63 Mn[Fe(CN)6]·1.41H2O.
[0086] S2, adding 2 mL of 0.015 M tannic acid aqueous solution, 1 mL of formaldehyde aqueous solution (3.7 wt %), 0.1 mL of ammonia water (25 wt %) and 3 mL of ethanol to 13 mL of deionized water, and mixing thoroughly to obtain a tannic acid precursor solution;
[0087] 0.15 g of Na 1.63Mn[Fe(CN)6]·1.41H2O was added to the tannic acid precursor solution, stirred continuously at 40°C for 24 h, filtered, and dried in vacuum at 80°C to obtain PB@TA.
[0088] S3, adding 0.3 g of octadecylamine into 20 mL of ethanol and fully dissolving it to obtain an octadecylamine precursor solution;
[0089] 0.15 g of PB@TA was added to the octadecylamine precursor solution, stirred continuously at 60°C for 24 h, filtered, and vacuum dried at 80°C to obtain the positive electrode material (PB@TA@ODA).
[0090] Example 3
[0091] The preparation method of the positive electrode material provided in this embodiment refers to that in embodiment 1, the only difference is that in step S2, Na 1.54 The mass of Fe[Fe(CN)6]·0.96H2O is 1g.
[0092] Example 4
[0093] The preparation method of the positive electrode material provided in this embodiment refers to that in embodiment 1, the only difference is that in step S2, Na 1.54 The mass of Fe[Fe(CN)6]·0.96H2O is 0.025g.
[0094] Example 5
[0095] The preparation method of the positive electrode material provided in this embodiment refers to that in Embodiment 1, the only difference is that in step S3, the mass of PB@TA is 3 g.
[0096] Example 6
[0097] The preparation method of the positive electrode material provided in this embodiment refers to that in Embodiment 1, except that in step S3, the mass of PB@TA is 0.06 g.
[0098] Example 7
[0099] The preparation method of the positive electrode material provided in this embodiment refers to that in embodiment 1, the only difference is that in step S2, Na 1.54 The mass of Fe[Fe(CN)6]·0.96H2O is 0.1 g. In step S3, the mass of PB@TA is 0.1 g.
[0100] Example 8
[0101] The preparation method of the positive electrode material provided in this embodiment refers to that in embodiment 1, the only difference is that in step S3, octadecylamine is replaced by octadecyl phosphate.
[0102] Example 9
[0103] The preparation method of the positive electrode material provided in this embodiment refers to that in embodiment 1, the only difference is that in step S3, octadecylamine is replaced by 1H,1H,2H,2H-perfluorodecanethiol.
[0104] Example 10
[0105] The preparation method of the positive electrode material provided in this embodiment refers to that in embodiment 1, the only difference is that in step S3, octadecylamine is replaced by N-phenylbistrifluoromethanesulfonic acid imide.
[0106] Comparative Example 1
[0107] The preparation method of the positive electrode material provided in this comparative example refers to Example 1, except that in step S2, no formaldehyde aqueous solution and ammonia water are added.
[0108] Comparative Example 2
[0109] The preparation method of the positive electrode material provided in this comparative example refers to Example 1, except that step S1 and step S2 are removed, and the Prussian blue matrix (PB) Na in Example 1 is 1.54 Fe[Fe(CN)6]·0.96H2O directly proceeds to step S3 to obtain the sample PB@ODA.
[0110] Test Example 1
[0111] XRD test was performed on PB and PB@TA@ODA in Example 1, and the results are as follows: Figure 1 shown.
[0112] from Figure 1 It can be seen that the structure of PB@TA@ODA has not changed significantly compared with that of PB, and it is still a pure cubic phase Prussian blue structure.
[0113] The PB@TA@ODA in Example 1 was tested by scanning electron microscopy, and the results are as follows: Figure 2 shown.
[0114] from Figure 2 It can be seen that PB@TA@ODA still maintains a cubic appearance.
[0115] Thermogravimetric tests were performed on PB, PB-7D, PB@TA@ODA and PB@TA@ODA-7D in Example 1. The results are as follows: Figure 3 and Figure 4 Among them, PB-7D means PB is placed at room temperature, pressure and 80% humidity for seven days, and PB@TA@ODA-7D means PB is placed at room temperature, pressure and 80% humidity for seven days.
[0116] from Figure 3 and Figure 4 It can be seen that the sample PB-7D loses weight significantly at 150℃ and 250℃, and the adsorbed water and interstitial water in the material increase significantly. The TG curve of PB@TA@ODA-7D is almost unchanged compared with PB@TA@ODA, showing excellent ability to inhibit hygroscopicity.
[0117] Test Example 2
[0118] The preparation method of the positive electrode plate includes the following steps: weigh the positive electrode material, the conductive agent (Ketjen Black and superconductive carbon black (Super P) with a mass ratio of 1:1) and polyvinylidene fluoride (PVDF) respectively according to a mass ratio of 7:2:1, add a certain amount of N-methylpyrrolidone (NMP) as a solvent, and grind into a uniform slurry. The above slurry is evenly coated on aluminum foil, and then baked at 70°C for 24 hours. Finally, it is cut into small discs with a diameter of 8mm to obtain a positive electrode plate. The positive electrode plate has a loading of 1.6 to 2.4 mg / cm 2 .
[0119] The preparation method of a sodium ion battery comprises the following steps: placing the above-mentioned positive electrode sheet into a 2032-type battery shell, using a sodium sheet as a negative electrode, glass fiber as a diaphragm, and nickel foam as a support sheet, wherein the electrolyte is 1 mol / L NaClO4 dissolved in EC (ethylene carbonate) and DEC (diethyl carbonate) in a volume ratio of 1:1, and 5% FEC (fluoroethylene carbonate) is added, and the assembly is performed in a glove box filled with argon gas, and the water content in the glove box is strictly controlled to be below 0.01 ppm and the oxygen content is below 0.05 ppm, so as to obtain a sodium ion battery.
[0120] The packaged sodium battery was placed at room temperature for 8 hours and then tested with a CT2001 charge and discharge tester from Wuhan Blue Electric Company. The charge and discharge voltage was set at 2.0V to 4.2V. In the cycle performance test, the battery was charged at 1C (1C = 170mA g -1 ) multiples for testing.
[0121] PB and PB@TA@ODA in Example 1 were respectively used as positive electrode materials, and positive electrode sheets were prepared according to the above-mentioned preparation method of positive electrode sheets. The wetting angle of the positive electrode sheets was tested, and the results are as follows: Figure 5 and Figure 6 shown.
[0122] from Figure 5 and Figure 6 It can be seen that Figure 5 The wetting angle of the positive electrode sheet made of PB is 108°; Figure 6The wetting angle of the positive electrode sheet made of PB@TA@ODA is 127°, which is much larger than that of the positive electrode sheet made of PB. It can be seen that PB@TA@ODA has good hydrophobicity.
[0123] PB, PB-7D, PB@TA@ODA and PB@TA@ODA-7D in Example 1 were respectively used as positive electrode materials, and sodium batteries were prepared according to the above-mentioned sodium ion battery preparation method. The sodium ion batteries were charged, discharged and cycled. The results are as follows: Figure 7 , Figure 8 , Fig. 9 and Fig.10 Among them, PB-7D means PB is placed at room temperature, pressure and 80% humidity for seven days, and PB@TA@ODA-7D means PB is placed at room temperature, pressure and 80% humidity for seven days.
[0124] From 7 and Figure 8 It can be seen that the first cycle discharge capacities of the sodium ion batteries made with PB and PB@TA@ODA are 142 mAh g -1 and 150mAh g -1 , there is no significant difference, and the cycle performance is relatively similar.
[0125] from Fig. 9 It can be seen that after PB was placed for seven days, the first cycle discharge capacity decayed to 116 mAh g -1 , its sodium storage performance decreased significantly; while the first cycle discharge capacity of PB@TA@ODA-7D was still 145 mAh g -1 As shown above, compared with PB@TA@ODA, there is almost no capacity attenuation, showing good storage properties under normal temperature, normal pressure and high humidity environment.
[0126] from Fig.10 It can be seen that the cycle stability of PB@TA@ODA-7D as the positive electrode of sodium ion battery is still very stable, showing a higher first-cycle efficiency and higher specific capacity, and exhibiting excellent hydrophobic properties.
[0127] The positive electrode materials prepared in Examples 1 to 10 and Comparative Examples 1 to 2 and the positive electrode materials after being placed for 7 days were respectively used to prepare sodium batteries according to the above-mentioned sodium ion battery preparation method. The sodium ion batteries were subjected to charge, discharge and cycle tests, and the results were recorded in Table 1.
[0128] Table 1
[0129]
[0130]
[0131] As can be seen from Table 1, Prussian blue can exhibit both excellent electrochemical performance and good environmental storage properties under the dual coating of a suitable amount of tannic acid polymer and a second layer of coating material.
[0132] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.
Claims
1. A positive electrode material, characterized in that: It comprises a Prussian blue matrix, and a first coating layer and a second coating layer sequentially coated on the surface of the Prussian blue matrix; The first coating layer is a polymer layer of tannic acid formed by the reaction of tannic acid, formaldehyde and ammonium ions; The material forming the second coating layer includes at least one of hexadecylamine, octadecylamine, octadecyl phosphate, N-phenylbistrifluoromethanesulfonic acid imide, 1H,1H,2H,2H-perfluorodecyltriethoxysilane and 1H,1H,2H,2H-perfluorodecylmercaptan; The thickness of the first coating layer is 3 to 4 nm; The thickness of the second coating layer is 1-2 nm.
2. The positive electrode material according to claim 1, characterized in that The chemical formula of the Prussian blue matrix is Na x M a M' b (CN)6·zH2O; wherein M and M' are each independently selected from at least one of Ni, Cu, Fe, Mn, Co and Zn, 0 <x<2,0<a<1,0<b<1,z> 0; And / or, the particle size of the positive electrode material is 200-300 nm.
3. The method for preparing the positive electrode material according to claim 1 or 2, characterized in that: The steps include: Mixing tannic acid, formaldehyde, ammonium ions, a first solvent and water to obtain a precursor solution containing tannic acid; The Prussian blue matrix and the precursor solution containing tannic acid undergo a first reaction to obtain PB@TA; The PB@TA, the material forming the second coating layer and the second solvent undergo a second reaction to obtain the positive electrode material.
4. The method for preparing the positive electrode material according to claim 3, characterized in that: The temperature of the first reaction and the second reaction is independently 25 to 80° C.; And / or, the time of the first reaction and the second reaction are each independently 1 to 72 hours.
5. The method for preparing the positive electrode material according to claim 3, characterized in that: The method comprises at least one of the following features (1) to (3); (1) The molar ratio of the tannic acid to the formaldehyde is (0.022-0.024):1; (2) the substance providing the ammonium ions includes aqueous ammonia; (3) The concentration of the ammonia water is 20-30 wt %, and the dosage ratio of the ammonia water to the tannic acid is 1 mL: 0.1-1 mmol.
6. The method for preparing the positive electrode material according to claim 3, characterized in that: The mass ratio of the Prussian blue matrix to the tannic acid is 1:(0.05-2); And / or, the mass ratio of the PB@TA to the material forming the second coating layer is 1:(0.1-5).
7. The method for preparing the positive electrode material according to claim 3, characterized in that: The first solvent includes ethanol; And / or, the second solvent includes at least one of methanol, ethanol, ethylene glycol, acetone and tetrahydrofuran.
8. A sodium ion battery, characterized in that: Comprising the positive electrode material according to claim 1 or 2.