A tellurium oxide-based solid electrolyte and preparation method thereof

By using Ba2+, Ca2+, Sr2+ and Te4+ doped with K+ or Co3+, Sb3+ in the perovskite solid electrolyte, and calcining and sintering in a low-temperature inert atmosphere, a tellurium oxide-based material is prepared, which solves the problem of element volatilization and price change during high-temperature sintering. problem, achieving high conductivity and catalytic activity, which is suitable for a variety of applications.

CN116874283BActive Publication Date: 2024-10-18NORTHEASTERN UNIV CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310847355.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-10
Publication Date
2024-10-18
Estimated Expiration
2043-07-10

AI Technical Summary

Technical Problem

Elements of existing perovskite solid electrolytes are severely volatilized during high-temperature sintering, resulting in reduced electrolyte performance. Cerium oxide and zirconium oxide-based materials are prone to price changes at high temperatures, requiring additional protection measures.

Method used

Ba2+, Ca2+, Sr2+ are used as A-site elements, Te4+ is used as B-site element, doped with K+ or Co3+, Sb3+, calcined and sintered in an inert atmosphere through low-temperature preparation method (500℃~900℃), and tellurium oxide powder is used to supplement tellurium element to prepare tellurium oxide-based ATeO3-based materials.

Benefits of technology

It reduces element volatilization, improves conductivity and catalytic activity, and is suitable for fields such as electrochemical synthesis, electrolysis of water for hydrogen production and hydrogen separation, reducing energy consumption and simplifying the preparation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116874283B_ABST
    Figure CN116874283B_ABST
Patent Text Reader

Abstract

A tellurium oxide-based solid electrolyte and a preparation method thereof, belonging to the technical field of solid electrolytes, the method of the invention adopts a +2 valent cation Ba 2+ , Ca 2+ or Sr 2+ As the A-site ion, select Te with a valence of +4 4+ ions as B-site elements to form ABO3 type materials, and K is doped at the A-site 1+ Elements or B-doped Co 3+ , Sb 3+ , we have prepared tellurium oxide-based proton conductor materials that have both high electrical conductivity and catalytic activity, which meet the application needs of proton conductors in the fields of electrochemical synthesis, water electrolysis to produce hydrogen, hydrogen separation, hydrogen measurement sensors, etc., and have good application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of solid electrolytes, and in particular relates to a tellurium oxide-based solid electrolyte and a preparation method thereof. Background Art

[0002] Perovskite solid electrolyte proton conductor is a functional material with protons as carriers. Perovskite proton conductor has broad application prospects in fuel cells, hydrogen sensors, hydrogen separation, hydrogen production, and ammonia synthesis.

[0003] ABO 3 The ideal crystal structure of a proton conductor is a cubic structure. However, with the replacement and doping of ions at the A and B positions, the change in the size of the ion radius and the change in the Coulomb force caused by the different charges carried by the ions will cause the crystal structure to shift and distort to a certain extent, deviating from the ideal cubic structure. Therefore, most perovskite proton conductors are orthorhombic, rhombic and tetragonal perovskite structures, in which the A position is usually a +2 cation (such as Ba 2+ , Ca 2+ ), B position is +4 cation (such as Zr 4+ 、Ce 4+ ), usually by doping the A-site or B-site element with a low-valent element to produce oxygen vacancies in the raw material. Oxygen vacancies capture water vapor or hydrogen in the atmosphere to generate protons, resulting in proton conductivity. Among them, materials with higher total ion conductivity (the sum of oxygen ion and proton conductivity) are suitable for use in fuel cells and water electrolysis to produce hydrogen; materials with higher proton conductivity and extremely low oxygen ion conductivity, that is, materials with higher proton migration numbers, are suitable for use in hydrogen separation, sensors and other fields.

[0004] Ceria-based and zirconia-based solid electrolytes are the most common ABO 3 Type solid electrolyte, Ce 4+ Ionic radius Zr 4+ Ionic radius Compared with Te 4+ Ionic radius Greater than Ce 4+ and Zr 4+ Therefore, using Te as the B-site element can make the optional ions at the B-site have a larger ionic radius. In addition, tellurium oxide has a smaller tolerance factor t (BaZrO 3 ,BaCeO 3 and BaTeO 3 For example, the allowable factors are 1, 0.938 and 0.898 respectively). The greater the deviation of the allowable factor t from 1, the greater the lattice distortion. Studies have shown that lattice distortion increases proton mobility, so tellurium oxide has a higher proton migration number.

[0005] In addition, the sintering preparation of cerium oxide and zirconium oxide-based solid electrolytes requires a high temperature of about 1600°C, which will cause the volatilization of some elements (such as Ba volatilization), resulting in reduced electrolyte performance; the sintering preparation temperature of tellurium oxide is about 800°C, which reduces element volatilization and saves energy. Since the Te element has many valence states and is prone to valence changes in a high-temperature oxygen-containing atmosphere, certain protective measures need to be taken during the sintering process. Summary of the invention

[0006] In view of the above problems, the present invention provides a tellurium oxide-based solid electrolyte and a medium-low temperature preparation method thereof, using Ba 2+ , Ca 2+ , Sr 2+ As ABO 3 The A-site element of the perovskite structure material is Te 4+ As the B-site element, K is doped into the A-site or Co and Sb are doped into the B-site to form ATeO 3 Base material.

[0007] The molecular formula of the tellurium oxide-based solid electrolyte of the present invention is A 1-x K x TeO 3-α or ATe 1-y B y O 3-α , the A-site element is selected from Ba, Ca and Sr, the B-site element is selected from Co and Sb, x=0~0.3, when x>0, it means that the A-site is doped with K element, y=0~0.3, and the value of 3-α is balanced with the total valence state.

[0008] The method for preparing the tellurium oxide-based solid electrolyte of the present invention comprises the following steps:

[0009] Method 1

[0010] (1) preparing oxides, carbonates or nitrates of elements A, B, K and Te as raw materials, wherein A is selected from Ba, Ca and Sr, and B is selected from Co and Sb;

[0011] (2) placing all the raw materials in a ball mill and adding anhydrous ethanol to mix by ball milling until the average particle size is ≤5 μm to obtain a mixed powder I;

[0012] (3) Pressing the mixed powder I into a block, placing tellurium oxide powder around it so that the tellurium oxide powder cannot contact the mixed powder I, covering it with a corundum crucible, and then calcining it in an inert atmosphere at 500° C. to 800° C. for 10 to 30 hours, cooling it to room temperature with the furnace, and obtaining a calcined material;

[0013] (4) placing the calcined material in a ball mill and grinding it to an average particle size of ≤5 μm to obtain a mixed powder II;

[0014] (5) The mixed powder II is pressed into a sheet, tellurium oxide powder is placed around it so that the tellurium oxide powder cannot come into contact with the mixed powder II, and the sheet is covered with a corundum crucible. The sheet is then sintered in an inert atmosphere at 600°C to 900°C for 5 to 30 hours, and the sheet is cooled to room temperature in the furnace to prepare a tellurium oxide-based solid electrolyte.

[0015] In the above step (1), the molecular formula is A 1-x K x TeO 3-α When the molar ratio of A, K and Te in all raw materials is (1-x):x:1, the molecular formula is ATe 1-y B y O 3-α The molar ratio of elements A, Te and B is 1:(1-y):y.

[0016] In the above step (3), the pressing pressure for pressing into blocks is 5 to 10 MPa.

[0017] In the above step (5), the pressing pressure for tableting is 100 to 300 MPa.

[0018] In the above steps (3) and (5), the calcination and sintering of the materials are carried out under an inert atmosphere.

[0019] In the above steps (3) and (5), placing tellurium oxide powder around the mixed powder can play a role in supplementing the tellurium element. The amount of the placed tellurium oxide powder is 5-25% of the weight of the target material.

[0020] Method 2

[0021] (1) preparing oxides, carbonates or nitrates of elements A, B, K and Te as raw materials, wherein A is selected from Ba, Ca and Sr, and B is selected from Co and Sb;

[0022] (2) placing all the raw materials in a ball mill and adding anhydrous ethanol to mix by ball milling until the average particle size is ≤5 μm to obtain a mixed powder I;

[0023] (3) Pressing the mixed powder I into a block, placing it in a closed tube furnace, calcining it at 500° C. to 800° C. in an inert atmosphere for 10 to 30 hours, and cooling it to room temperature with the furnace to obtain a calcined material;

[0024] (4) placing the calcined material in a ball mill and grinding it to an average particle size of ≤5 μm to obtain a mixed powder II;

[0025] (5) The mixed powder II is pressed into a sheet, and then placed in a closed tubular furnace, sintered at 600°C to 900°C in an inert atmosphere for 5 to 30 hours, and cooled to room temperature in the furnace to prepare a tellurium oxide-based solid electrolyte.

[0026] In the above step (1), an excess of 5 to 10% of tellurium oxide having a molecular formula of A is added. 1-x K x TeO 3-α The molar ratio of A, K and Te in all raw materials is (1-x):x:(1.05~1.1), and the molecular formula is ATe 1-y B y O 3-α When the molar ratio of A, Te and B elements is 1:((1.05~1.1)-y):y.

[0027] In the above step (3), the pressing pressure for pressing into blocks is 5 to 10 MPa.

[0028] In the above step (5), the pressing pressure for tableting is 100 to 300 MPa.

[0029] In the above steps (3) and (5), the calcination and sintering of the materials are carried out under an inert atmosphere.

[0030] Beneficial effects of the present invention:

[0031] The method of the present invention adopts +2 cation Ba 2+ , Ca 2+ or Sr 2+ As the A-site ion, select Te with a valence of +4 4+ Ion is the B-site element, forming ABO 3 Type material, and doped with K at the A position 1+ Elements or B-doped Co 3+ , Sb 3+ , we have prepared tellurium oxide-based proton conductor materials that have both high electrical conductivity and catalytic activity, which meet the application needs of proton conductors in the fields of electrochemical synthesis, water electrolysis to produce hydrogen, hydrogen separation, hydrogen measurement sensors, etc., and have good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 is Ba in Example 1 of the present invention 0.9 K 0.1 TeO 3-α XRD of solid electrolyte.

[0033] Figure 2 is BaTe in Example 2 of the present invention 0.9 Co 0.1 O 3XRD of solid electrolytes.

[0034] Figure 3 The tellurium oxide solid electrolyte in the embodiment of the present invention is heated to 500-700°C and 1% H 2 The rest are Arrhenius curves of conductivity under argon atmosphere conditions; ■ in the figure is Example 1, and ● is Example 2.

[0035] Figure 4 is Ba in Example 1 of the present invention 0.9 K 0.1 TeO 3-α The proton transfer number of the solid electrolyte. DETAILED DESCRIPTION

[0036] The raw materials used in the examples of the present invention are commercially available analytically pure reagents.

[0037] The grinding jar used in the embodiment of the present invention is made of agate.

[0038] In the embodiment of the present invention, calcination and sintering are both carried out in a silica tube furnace in an inert atmosphere. A hose is connected to one end of the tube furnace and placed in water to ensure that the pressure in the gas expansion tube is not too high when heated to high temperature, and argon is appropriately introduced when cooling to prevent water from being sucked back into the furnace tube.

[0039] The conductivity of the mixed solid electrolyte proton conductor material in the embodiment of the present invention is ≤1.0×10 -4 S / cm.

[0040] In the embodiment of the present invention, when the mixed powder II is pressed into tablets, an isostatic pressing device is used for synthetic pressing.

[0041] The raw materials in the embodiments of the present invention are carbonates or oxides of the elements Ba, Co, K, Sb and Te.

[0042] Example 1

[0043] A tellurium oxide-based solid electrolyte with the molecular formula Ba 0.9 K 0.1 TeO 3-α ;

[0044] The method for preparing the tellurium oxide-based solid electrolyte comprises the following specific steps:

[0045] Preparation of TeO 2 , K 2 CO 3 and BaCO 3 The powder is the raw material; the molar ratio of Ba, K and Te elements in all the raw materials is 0.9:0.1:1;

[0046] All raw materials were placed in a ball mill and anhydrous ethanol was added to mix by ball milling until the average particle size was ≤5 μm, to obtain mixed powder I;

[0047] The mixed powder I is pressed into blocks by a tablet press at a pressing pressure of 5 MPa, tellurium oxide powder is placed around the mixed powder I block to supplement the Te element but not in contact with it, and is covered with a corundum crucible, and then placed in a high-temperature tube furnace for calcination at 700° C. in an argon atmosphere for 15 hours, and cooled to room temperature with the furnace to obtain a calcined material; wherein the amount of tellurium oxide powder placed is about 10% of the weight of the target material;

[0048] The calcined material is placed in a ball mill and ground to an average particle size of ≤5 μm to obtain a mixed powder II;

[0049] The mixed powder II was pressed into a tablet using an isostatic pressing device at a pressing pressure of 200 MPa and constant pressure for 10 min. Tellurium oxide powder was placed around to supplement the Te element. The tablet was covered with a corundum crucible and then placed in an argon-filled tubular furnace. The tablet was sintered at 830°C for 20 hours and cooled to room temperature to prepare a tellurium oxide-based solid electrolyte. XRD results are as follows: Figure 1 As shown, the migration number is Figure 4 The tellurium oxide solid electrolyte is heated to 500-700°C and 1% H 2 The rest are the conductivity Arrhenius curves under argon atmosphere conditions. Figure 3 shown.

[0050] Example 2

[0051] A tellurium oxide-based solid electrolyte with the molecular formula BaTe 0.9 Co 0.1 O 3-α ;

[0052] The method for preparing the tellurium oxide-based solid electrolyte comprises the following specific steps:

[0053] Preparation of TeO 2 、BaCO 3 、Co 2 O 3 The powder is used as the raw material; the molar ratio of Ba, Te and Co in all the raw materials is 1:0.95:0.1; all the raw materials are placed in a ball mill and anhydrous ethanol is added to mix by ball milling until the average particle size is ≤5 μm, thereby obtaining a mixed powder I;

[0054] The mixed powder I was pressed into blocks using a tablet press at a pressing pressure of 6 MPa, and then calcined in an argon atmosphere at 700° C. for 10 hours using a high-temperature tube furnace, and then cooled to room temperature with the furnace to obtain a calcined material;

[0055] The calcined material is placed in a ball mill and ground to an average particle size of ≤5 μm to obtain a mixed powder II;

[0056] The mixed powder II was pressed into a tablet using an isostatic pressing device at a pressing pressure of 200 MPa and constant pressure for 10 min. The tablet was then placed in a tubular furnace filled with argon and sintered at 850 ° C for 20 hours. The tablet was cooled to room temperature to prepare a tellurium oxide-based solid electrolyte. XRD results showed that Figure 2 As shown, the migration number is Figure 4 As shown; the tellurium oxide solid electrolyte is at a temperature of 500-700°C and 1% H 2 The rest are the conductivity Arrhenius curves under argon atmosphere conditions. Figure 3 shown.

[0057] Example 3

[0058] A tellurium oxide-based solid electrolyte with a molecular formula of Ca 0.9 K 0.1 TeO 3-α ;

[0059] The preparation method of the tellurium oxide-based solid electrolyte is the same as that of Example 1, except that:

[0060] (1) The molar ratio of Ca, K and Te in all raw materials is 0.9:0.1:1;

[0061] (2) The conductivity of tellurium oxide-based solid electrolyte at 700°C is 1.2×10 -4 S / cm.

[0062] Example 4

[0063] A tellurium oxide-based solid electrolyte with the molecular formula BaTe 0.9 Sb 0.1 O 3-α ;

[0064] The preparation method of the tellurium oxide-based solid electrolyte is the same as that of Example 2, except that:

[0065] (1) Preparation of TeO 2 、BaCO 3 , Sb 2 O 3 The powder is the raw material, and the molar ratio of Ba, Te and Sb in all the raw materials is 1:0.95:0.1;

[0066] (2)BaTe 0.9 Sb 0.1 O 3-α The conductivity of the solid electrolyte at 700°C is 1.0×10 -4S / cm.

[0067] Example 5

[0068] A tellurium oxide-based solid electrolyte with the molecular formula of CaTe 0.9 Co 0.1 O 3-α ;

[0069] The preparation method of the tellurium oxide-based solid electrolyte is the same as that of Example 2, except that:

[0070] (1) Preparation of TeO 2 、CaCO 3 、Co 2 O 3 The powder is used as raw material, and the molar ratio of Ca, Te and Co in all raw materials is 1:0.95:0.1;

[0071] (2)CaTe 0.9 Co 0.1 O 3-α The conductivity of tellurium oxide-based solid electrolyte at 700°C is 1.1×10 -4 S / cm.

[0072] Example 6

[0073] A tellurium oxide-based solid electrolyte with the molecular formula BaTeO 3 ;

[0074] The preparation method of the tellurium oxide-based solid electrolyte is the same as that of Example 1, except that:

[0075] (1) Preparation of TeO 2 、BaCO 3 The powder is the raw material, and the molar ratio of Ba to Te in all the raw materials is 1:1;

[0076] (2)BaTeO 3 The conductivity of the solid electrolyte at 700°C is 4.2×10 -6 S / cm.

Claims

1. A tellurium oxide-based solid electrolyte, characterized in that: The tellurium oxide-based solid electrolyte has the molecular formula A 1- x K x TeO 3-α or ATe 1-y B y O 3-α ; Among them, the A-site element is selected from Ba, Ca and Sr, the B-site element is selected from Co and Sb, x=0.1~0.3, y=0.1~0.3, and the value of 3-α is balanced with the total valence state; x>0 indicates that the A-site is doped with K element.

2. The method for preparing a tellurium oxide-based solid electrolyte according to claim 1, characterized in that: The steps include: (1) preparing oxides, carbonates or nitrates of elements A, B, K and Te as raw materials, wherein A is selected from Ba, Ca and Sr, and B is selected from Co and Sb; (2) placing all the raw materials in a ball mill and adding anhydrous ethanol to mix by ball milling until the average particle size is ≤5 μm to obtain a mixed powder I; (3) Pressing the mixed powder I into a block, placing tellurium oxide powder around it so that the tellurium oxide powder cannot contact the mixed powder I, covering it with a corundum crucible, and then calcining it in an inert atmosphere at 500° C. to 800° C. for 10 to 30 hours, cooling it to room temperature with the furnace, and obtaining a calcined material; (4) placing the calcined material in a ball mill and grinding it to an average particle size of ≤5 μm to obtain a mixed powder II; (5) The mixed powder II is pressed into a sheet, tellurium oxide powder is placed around it so that the tellurium oxide powder cannot come into contact with the mixed powder II, and the sheet is covered with a corundum crucible. The sheet is then sintered in an inert atmosphere at 600°C to 900°C for 5 to 30 hours, and the sheet is cooled to room temperature in the furnace to prepare a tellurium oxide-based solid electrolyte.

3. The method for preparing a tellurium oxide-based solid electrolyte according to claim 2, characterized in that: In the step (1), the molecular formula is A 1-x K x TeO 3-α The molar ratio of A, K and Te in all raw materials is (1-x):x:1, and the molecular formula is ATe 1-y B y O 3-α The molar ratio of elements A, Te and B is 1:(1-y):y.

4. The method for preparing a tellurium oxide-based solid electrolyte according to claim 2, characterized in that: In the step (3), the pressing pressure for pressing into blocks is 5 to 10 MPa.

5. The method for preparing a tellurium oxide-based solid electrolyte according to claim 2, characterized in that: In the step (5), the pressing pressure for tableting is 100 to 300 MPa.

6. The method for preparing a tellurium oxide-based solid electrolyte according to claim 2, characterized in that: In the steps (3) and (5), the calcination and sintering of the materials are both carried out under an inert atmosphere.

7. The method for preparing a tellurium oxide-based solid electrolyte according to claim 1, characterized in that: The steps include: (1) preparing oxides, carbonates or nitrates of elements A, B, K and Te as raw materials, wherein A is selected from Ba, Ca and Sr, and B is selected from Co and Sb; (2) placing all the raw materials in a ball mill and adding anhydrous ethanol to mix by ball milling until the average particle size is ≤5 μm to obtain a mixed powder I; (3) Pressing the mixed powder I into a block, placing it in a closed tube furnace, calcining it at 500° C. to 800° C. in an inert atmosphere for 10 to 30 hours, and cooling it to room temperature with the furnace to obtain a calcined material; (4) placing the calcined material in a ball mill and grinding it to an average particle size of ≤5 μm to obtain a mixed powder II; (5) The mixed powder II is pressed into a sheet, and then placed in a closed tubular furnace, sintered at 600°C to 900°C in an inert atmosphere for 5 to 30 hours, and cooled to room temperature in the furnace to prepare a tellurium oxide-based solid electrolyte.

8. The method for preparing a tellurium oxide-based solid electrolyte according to claim 7, characterized in that: In the step (1), an excess of 5 to 10% of tellurium oxide having a molecular formula of A is added. 1-x K x TeO 3-α The molar ratio of A, K and Te in all raw materials is (1-x):x:(1.05~1.1), and the molecular formula is ATe 1-y B y O 3-α When the molar ratio of A, Te and B elements is 1:((1.05~1.1)-y):y.

9. The method for preparing a tellurium oxide-based solid electrolyte according to claim 7, characterized in that: In the step (3), the pressing pressure for pressing into blocks is 5 to 10 MPa; in the step (5), the pressing pressure for pressing into tablets is 100 to 300 MPa.

10. The method for preparing a tellurium oxide-based solid electrolyte according to claim 7, characterized in that: In the steps (3) and (5), the calcination and sintering of the materials are both carried out under an inert atmosphere.