Environmentally friendly lead-free glass glaze coating, ZnO varistor side insulating coating and preparation method thereof
Through lead-free glass glaze coating and vitrification heat treatment technology, the problems of poor adhesion and insufficient temperature resistance of ZnO resistor insulating materials are solved, and the insulation coating with high adhesion, impact resistance and environmental protection are achieved, and the lightning arrester is improved and surge protector reliability and reduce environmental pollution.
Patent Information
- Application Number
- CN202310908777.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-24
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-07-24
AI Technical Summary
The insulating materials of existing ZnO resistor sheets, especially organic epoxy resin paint and lead-containing glass glaze materials, have problems such as poor adhesion, insufficient temperature resistance and solvent irritating odor, which affects the reliability of lightning arresters and surge protectors. and environmentally friendly.
Lead-free glass glaze coating is used, and the composition includes PEG20000, lead-free glass powder, ethanol and water. By preheating spraying and glass-transforming heat treatment, a uniform and dense insulating coating is formed, which solves the problem of insufficient adhesion and temperature resistance. , and replace traditional organic solvents with a mixed solvent of water and ethanol, reducing irritating odors.
The high adhesion, high current impact resistance and environmental protection of the side insulation coating of the ZnO resistor sheet are achieved, the reliability of the lightning arrester and surge protector is improved, and the use of harmful substances and environmental pollution in the production process is reduced.
Smart Images

Figure BDA0004354417010000081 
Figure BDA0004354417010000091 
Figure HDA0004354417020000011
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ZnO varistor sheets for lightning arresters and ZnO varistor sheets for surge protectors, and in particular relates to an environmentally friendly lead-free glass glaze coating, a side insulating coating of a ZnO varistor sheet and a preparation method thereof. Background Art
[0002] The electric power industry is the most important basic energy industry in the development of the national economy, the first basic industry of the national economy, and the priority development focus in the economic development strategies of countries around the world. Strengthening the construction of smart grids is an important guiding ideology for the reform and development of my country's electric power industry, and it is also the future development trend of the world's electric power industry. Lightning arresters and surge protectors are key equipment for human lightning protection and disaster reduction. They are widely used for their superior protection performance, pollution resistance, and stable performance. As an indispensable electrical equipment in the construction of smart grids, they are inseparable from the development of the electric power industry.
[0003] As the core component of lightning arresters and surge protectors, the performance of ZnO resistors determines the performance of lightning arresters and surge protectors. In order to prevent the ZnO resistor from flashing along the side under high voltage and high current impact, a layer of insulation with excellent insulation must be applied to the side of the ZnO resistor body so that the side of the ZnO resistor body will not be broken down by the large surge current and fail.
[0004] At present, the most widely used insulating materials in the ZnO resistor industry at home and abroad are organic epoxy resin paint and inorganic glass glaze materials. Organic epoxy resin paint has good molding characteristics and chemical stability. However, due to the large difference in thermal expansion coefficient between organic epoxy resin paint and ZnO resistor, its adhesion to the ZnO resistor body is poor, and its temperature resistance is also poor. Carbonization will occur above 190°C. When the ZnO resistor encounters a large surge current shock, its body temperature will quickly rise from room temperature to about 150-300°C. After being subjected to thermal shock, the organic epoxy resin paint is easy to peel off from the ZnO resistor body, and the coating will fall off, and the side electrical insulation performance will be lost, which seriously affects the reliability of the arrester or surge protector. The thermal expansion coefficient of inorganic glass glaze can be adjusted, and it has excellent bonding with the ZnO resistor body, and its temperature resistance is very good, up to 500°C or more. Therefore, the use of inorganic glass glaze material is an effective solution for improving the side insulation performance of ZnO resistors at home and abroad.
[0005] At present, the inorganic glass glaze used in the ZnO resistor industry at home and abroad is mostly leaded glass with a lead content of 60-70%, and the solvents used are volatile and have a strong pungent odor, such as diethylene glycol butyl ether, butyl acetate and other organic substances as solvents, which cause certain pollution to human health and the atmospheric environment. Summary of the invention
[0006] The purpose of the present invention is to provide an environmentally friendly lead-free glass glaze coating, a ZnO varistor sheet side insulating coating and a preparation method thereof. The lead-free glass glaze coating of the present invention is environmentally friendly and lead-free, has no irritating odor during use, and has a more uniform coating and better resistance to large current impacts.
[0007] The present invention provides an environmentally friendly lead-free glass enamel coating, comprising the following components in percentage by mass:
[0008] PEG20000: 2%~5%, lead-free glass powder: 60%~75%, ethanol: 15%~30%, water: 8%~20%.
[0009] Preferably, the environmentally friendly lead-free glass enamel paint comprises the following components in percentage by mass:
[0010] PEG20000: 2%~3.5%, lead-free glass powder: 65%~75%, ethanol: 18%~25%, water: 10%~15%.
[0011] Preferably, the lead-free glass powder comprises the following components in mass fractions: bismuth: 74±5.0%, silicon: 3.7±0.5%, boron: 2.8±0.3%, zinc: 11.6±1.0%, aluminum: 2.60±0.3%, lithium: 0.8±0.1%, and copper: 4.5±0.6%.
[0012] The present invention provides a method for preparing a side insulating coating of a ZnO varistor sheet, comprising the following steps:
[0013] A) Preheating the ZnO varistor to 80-150°C, then spraying the environmentally friendly lead-free glass glaze paint on the side of the ZnO varistor, using the temperature of the preheated ZnO varistor itself to dry the side paint without sagging, to obtain a paint layer;
[0014] The environmentally friendly lead-free glass enamel paint is the environmentally friendly lead-free glass enamel paint in claim 1 or 2;
[0015] B) subjecting the coating layer to a vitrification heat treatment to obtain a side insulating coating of the ZnO varistor sheet.
[0016] Preferably, the thickness of the insulating coating on the side of the ZnO varistor sheet is 150-250 μm.
[0017] Preferably, the vitrification heat treatment process is:
[0018] The temperature is raised from room temperature to 350°C at a rate of 0.5-2.5°C / min, and kept at 350°C for 1-4 hours to remove binder. After the insulation, the temperature is raised to 450-550°C at a rate of 1.0-1.5°C / min and kept for 1-2 hours to obtain the insulating coating on the side of the ZnO varistor sheet.
[0019] Preferably, the vitrification heat treatment process is:
[0020] The temperature is raised from room temperature to 350°C at a rate of 1-2.5°C / min, and kept at 350°C for 2 hours to remove binder. After the insulation, the temperature is raised to 450-550°C at a rate of 1.0-1.5°C / min and kept for 1 hour to obtain the insulating coating on the side of the ZnO varistor.
[0021] Preferably, the spraying in step A) is electrostatic spraying or slurry spraying.
[0022] Preferably, the environmentally friendly lead-free glass glaze coating is prepared according to the following steps:
[0023] PEG20000, water and ethanol are mixed, and then lead-free glass powder is added, and the mixture is evenly stirred and ball-milled for 2 to 6 hours to obtain an environmentally friendly lead-free glass glaze coating.
[0024] The present invention provides a side insulating coating of a ZnO varistor sheet prepared by the preparation method described above.
[0025] The present invention provides an environmentally friendly lead-free glass glaze coating, comprising the following components in mass percentage: PEG20000: 2% to 5%, lead-free glass powder: 60% to 75%, ethanol: 15% to 30%, and water: 8% to 20%. All components of the present invention do not contain harmful substances, and the use is environmentally friendly, reliable and safe. In addition, the process method for preparing the glass glaze coating of the present invention is simple and has high production efficiency. After all the components are mixed together, they can be used after ball milling for more than 2 hours. Compared with the glass glaze coating that can only be sprayed with slurry in the prior art, the glass glaze coating can be sprayed with slurry or electrostatically, and can be matched with a spraying device to realize automatic spraying. The material loading rate of one spraying can reach more than 60%, and the coating sprayed outside the workpiece can be recycled and reused, and the comprehensive utilization rate of materials is as high as more than 80%. The glass glaze coating of the present invention is applied on the ZnO resistor, and after heat treatment, a coating with uniform and dense thickness and smooth appearance is formed. The coating is thinner and more uniform, and the finished ZnO resistor has good waterproofness, antifouling property, and high insulation performance, which can effectively improve the high current impact resistance of the ZnO resistor. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0027] Figure 1 is the heat treatment temperature curve used in Example 1 of the present invention;
[0028] Figure 2 This is an electron microscope image of the insulating coating with a glaze layer thickness of 90 μm in Example 3 (magnified 100 times);
[0029] Figure 3 This is an electron microscope image of the insulating coating with a glaze layer thickness of 160 μm in Example 3 (magnified 100 times). DETAILED DESCRIPTION
[0030] The present invention provides an environmentally friendly lead-free glass enamel coating, comprising the following components in percentage by mass:
[0031] PEG20000: 2%~5%, lead-free glass powder: 60%~75%, ethanol: 15%~30%, water: 8%~20%.
[0032] In the present invention, the lead-free glass powder includes the following components by mass fraction: Bi / bismuth: 74±5.0%, Si / silicon: 3.7±0.5%, B / boron: 2.8±0.3%, Zn / zinc: 11.6±1.0%, Al / aluminum: 2.60±0.3%, Li / lithium: 0.8±0.1%, Cu / copper: 4.5±0.6%. Specifically, in an embodiment of the present invention, the lead-free-B type lead-free glass powder produced by Xi'an Zhenxin Electronic Technology Co., Ltd. can be used.
[0033] In the present invention, the mass percentage of the lead-free glass powder is preferably 60% to 75%, more preferably 65% to 70%, such as 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, preferably a range value with any of the above values as the upper or lower limit.
[0034] In the present invention, the solvent of the environmentally friendly lead-free glass glaze coating is a mixed solvent of water and ethanol, and the mass percentage of water is preferably 8% to 20%, more preferably 10% to 15%, such as 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, preferably a range value with any of the above values as the upper or lower limit; the mass percentage of ethanol is preferably 15% to 30%, more preferably 18% to 25%, such as 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, preferably a range value with any of the above values as the upper or lower limit.
[0035] In the present invention, the polyethylene glycol 20000 (PEG20000) is used as a water-soluble adhesive, and its mass percentage is preferably 2% to 5%, more preferably 2% to 3.5%, such as 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, preferably a range value with any of the above values as the upper or lower limit. The present invention has found that in order to solve the problem of pungent odor of the coating, a mixed solution of water and ethanol is used as a solvent for the glass glaze coating, but in the water-soluble coating system, not some conventional water-soluble adhesives are suitable for the lead-free glass glaze system in this application, such as hydroxyethyl cellulose, etc. The present invention uses PEG20000 to meet the preparation of the coating and the subsequent spraying and vitrification process.
[0036] The present invention also provides a method for preparing a side insulating coating of a ZnO varistor sheet, comprising the following steps:
[0037] A) Preheating the ZnO varistor to 80-150°C, then spraying the environmentally friendly lead-free glass glaze paint on the side of the ZnO varistor, using the temperature of the preheated ZnO varistor itself to dry the side paint without sagging, to obtain a paint layer;
[0038] The environmentally friendly lead-free glass glaze paint is the environmentally friendly lead-free glass glaze paint mentioned above;
[0039] B) subjecting the coating layer to a vitrification heat treatment to obtain a side insulating coating of the ZnO varistor sheet.
[0040] Since the glass enamel coating used in the present invention is a water-soluble system, the volatility of water is poor compared with that of organic solvents such as butyl acetate, and the vaporization temperature range is very narrow, and the evaporation rate of water is too fast. Therefore, the present application preheats the ZnO varistor sheet first, and needs to preheat it within a relatively low temperature range, preferably 80-150°C, more preferably 100-150°C, such as 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, preferably with any of the above values as the upper or lower limit of the range value.
[0041] In the present invention, the lead-free glass glaze coating is obtained by mixing various components and then ball milling, and the specific steps are as follows:
[0042] PEG20000, water and ethanol are mixed, and then lead-free glass powder is added, and the mixture is evenly stirred and ball-milled for 2 to 6 hours to obtain an environmentally friendly lead-free glass glaze coating.
[0043] In the present invention, the environmentally friendly lead-free glass glaze coating can be achieved by electrostatic spraying or slurry spraying. The present invention is described by taking slurry spraying as an example.
[0044] In the present invention, after the environmentally friendly lead-free glass glaze paint is sprayed onto the side pieces of the resistor, the paint sprayed on the side pieces is dried by the temperature of the resistor after preheating without causing sagging, thereby forming a paint layer.
[0045] Then the coating layer is subjected to vitrification heat treatment, and the specific treatment process is as follows:
[0046] The temperature is raised from room temperature to 350°C at a rate of 0.5-2.5°C / min, and kept at 350°C for 1-4 hours to remove binder. After the insulation, the temperature is raised to 450-550°C at a rate of 1.0-1.5°C / min and kept for 1-2 hours to obtain the insulating coating on the side of the ZnO varistor sheet.
[0047] Preferably, in order to improve the efficiency of heat treatment while ensuring precise control of heat treatment temperature, the temperature can be first raised from room temperature to 150°C at a faster rate of 1-2.5°C / min to improve efficiency, and then raised to 350°C at a slower rate of 0.5-2°C / min to ensure sufficient debinding time.
[0048] Preferably, the temperature is increased from room temperature to 150°C at a rate of 2.0°C / min, then increased to 350°C at a rate of 1°C / min, and kept at 350°C for 2 hours to perform binder removal. After the insulation is completed, the temperature is increased to 450-550°C at a rate of 1.0-1.5°C / min and kept for 1 hour to obtain the insulating coating on the side of the ZnO varistor sheet.
[0049] In order to ensure the accuracy of temperature control during the insulation period, the present invention preferably first heats the temperature from 350°C to 480°C at a rate of 1.5-1.8°C / min, then heats the temperature to 485-550°C at a rate of 1.0-1.5°C / min and keeps warm for 1 hour, preferably heats the temperature to 490-540°C, such as 485°C, 490°C, 495°C, 500°C, 505°C, 510°C, 515°C, 520°C, 525°C, 530°C, 535°C, 540°C, 545°C, 550°C, preferably with any of the above values as the upper or lower limit of the range value.
[0050] The present invention also provides an insulating coating on the side of a ZnO varistor sheet prepared according to the preparation method described above, wherein the thickness of the coating is 150 to 300 μm. Compared with the insulating coating in the prior art, the coating in the present invention has better uniformity, higher insulation strength, and can achieve excellent resistance to large current impacts.
[0051] In the present invention, the insulating coating or the environmentally friendly lead-free glass glaze coating is applied to ZnO varistor sheets for lightning arresters and ZnO varistor sheets for surge protectors.
[0052] The present invention provides an environmentally friendly lead-free glass glaze coating, which is a mixture of a water-soluble and alcohol-soluble adhesive with water and ethanol in a certain proportion as a solvent, and then mixed with lead-free glass powder to form a glass glaze coating. Compared with the glass glaze coating currently used in the industry as a solvent and made from a mixture of ethyl cellulose, butyl acetate and dibutyl ether, the dissolution time is long, it is easy to volatilize and accompanied by a pungent odor, it is not environmentally friendly and will cause certain personal injuries. The coating solvent of the present invention is easy to dissolve, colorless and odorless, not volatile, non-toxic and harmless. The glass glaze coating prepared by the solvent prepared by the method, after being coated on a resistor and subjected to heat treatment, has a dense glass glaze layer, a smooth surface, excellent insulation performance and is easy to control during preparation and use. It effectively solves the shortcomings of conventional glass glaze coatings prepared with organic solvents, such as being easy to volatilize, toxic and harmful, and not environmentally friendly.
[0053] In order to further illustrate the present invention, an environmentally friendly lead-free glass glaze coating, a ZnO varistor sheet side insulating coating and a preparation method thereof provided by the present invention are described in detail below in combination with embodiments, but it should not be construed as limiting the scope of protection of the present invention.
[0054] Example 1
[0055] An environmentally friendly lead-free glass glaze coating for the side insulation of a ZnO resistor comprises the following components in weight percentage: PEG20000 2.0%, pure water 14%, CH3CH2OH 24%, and lead-free glass powder 60%. The lead-free glass powder comprises: Bi / bismuth: 74±5.0%, Si / silicon: 3.7±0.5%, B / boron: 2.8±0.3%, Zn / zinc: 11.6±1.0%, Al / aluminum: 2.60±0.3%, Li / lithium: 0.8±0.1%, and Cu / copper: 4.5±0.6%.
[0056] Pour PEG20000 into pure water and CH3CH2OH according to the above weight percentage with water and ethanol, stir and dissolve to form a mixed solution, then pour the corresponding proportion of lead-free glass powder into the mixed solution and stir evenly, and then after ball milling in a stirring ball mill for 2 hours, an environmentally friendly glass glaze coating is formed.
[0057] The resistor to be sprayed is first heated to 80-150℃ using a customized automatic spraying device, and then the prepared glass glaze paint is evenly sprayed on the side of the resistor using a spray gun. The temperature after the resistor is heated is used to dry the paint sprayed on the side without causing sagging.
[0058] according to Figure 1 The vitrification heat treatment was carried out according to the heat treatment temperature curve in , specifically: the temperature was increased from room temperature to 150°C at a rate of 2.0°C / min, then increased to 350°C at a rate of 1°C / min, kept at 350°C for 2 hours, and debinding was carried out. After the insulation, the temperature was increased to 515°C at a rate of 1.4°C / min and kept for 1 hour. After the insulation, the temperature was lowered to room temperature at a rate of 1.5-2.0°C / min.
[0059] Example 2
[0060] The insulating coating on the side of the ZnO varistor sheet prepared according to the method in Example 1 is different in that the environmentally friendly lead-free glass glaze coating in Example 2 includes the following components in weight percentage: PEG20000 2.0%, pure water 11%, CH3CH2OH 22%, and lead-free glass powder 65%.
[0061] Example 3
[0062] The insulating coating on the side of the ZnO varistor sheet prepared according to the method in Example 1 is different in that the environmentally friendly lead-free glass glaze coating in Example 3 includes the following components in weight percentage: PEG20000 2.0%, pure water 9%, CH3CH2OH 18%, and lead-free glass powder 70%.
[0063] Example 4
[0064] The insulating coating on the side of the ZnO varistor sheet prepared according to the method in Example 1 is different in that the environmentally friendly lead-free glass glaze coating in Example 4 includes the following components in weight percentage: PEG20000 2.5%, pure water 14%, CH3CH2OH 23.5%, and lead-free glass powder 60%.
[0065] Example 5
[0066] The insulating coating on the side of the ZnO varistor sheet prepared according to the method in Example 1 is different in that the environmentally friendly lead-free glass glaze coating in Example 5 includes the following components in weight percentage: PEG20000 2.5%, pure water 11%, CH3CH2OH 21.5%, and lead-free glass powder 65%.
[0067] Example 6
[0068] The insulating coating on the side of the ZnO varistor sheet prepared according to the method in Example 1 is different from that in Example 6, the environmentally friendly lead-free glass glaze coating includes the following components in weight percentage: PEG20000 2.5%, pure water 9%, CH3CH2OH 17.5%, and lead-free glass powder 70%.
[0069] Example 7
[0070] The insulating coating on the side of the ZnO varistor sheet prepared according to the method in Example 1 is different from that in Example 7, the environmentally friendly lead-free glass glaze coating includes the following components in weight percentage: PEG20000 3.0%, pure water 14%, CH3CH2OH 23%, and lead-free glass powder 60%.
[0071] Example 8
[0072] The insulating coating on the side of the ZnO varistor sheet prepared according to the method in Example 1 is different in that the environmentally friendly lead-free glass glaze coating in Example 8 includes the following components in weight percentage: PEG20000 3.0%, pure water 11%, CH3CH2OH 21%, and lead-free glass powder 65%.
[0073] Example 9
[0074] The insulating coating on the side of the ZnO varistor sheet prepared according to the method in Example 1 is different from that in Example 9, the environmentally friendly lead-free glass glaze coating includes the following components in weight percentage: PEG20000 3.0%, pure water 9%, CH3CH2OH 18%, and lead-free glass powder 70%.
[0075] The side insulating coatings of the ZnO varistor sheets prepared in Examples 1 to 9 were tested for electrical insulation performance of the varistor sheets: the test method was carried out according to the high current impact withstand test in GB / T 11032. Table 1 shows the test results.
[0076] Table 1 High current impact tolerance performance of the insulating coating on the side of the ZnO varistor in Examples 1 to 9
[0077]
[0078] According to the preparation method in Example 3, 5 insulating coatings with different glaze layer thicknesses (1# to 4#) were prepared, and each insulating coating with different thickness was tested 5 times in parallel (NO.1 to NO.20), and the test method was carried out according to the high current impulse withstand test in GB / T11032. The results are shown in Table 2.
[0079] Table 2 High current impact tolerance performance of insulating coatings of different thicknesses in Example 3
[0080]
[0081] Through experimental research, this application determines the correlation between the spray weight and the glaze layer thickness by setting an empirical coefficient, as shown in Table 2. Taking the glaze layer of about 90 μm thick as an example, the value of the spray weight (in g) is the lateral area of the ZnO varistor (in cm 2 Calculation) × empirical coefficient (0.065), such as Figures 2-3 As shown, Figure 2 This is an electron microscope picture (magnified 100 times) of the insulating coating sprayed with a weight of 2.3 g in Example 3 of the present invention. Figure 3 This is an electron microscope picture (magnified 100 times) of the insulating coating with a spray weight of 3.1g in Example 3 of the present invention. The ZnO varistor used in the embodiment of the present invention is model D45H24, with a side area of 36cm 2 , when the spray weight is 2.3g and 3.1g respectively, Figure 2 and Figure 3 It can be seen that the thickness of the coatings obtained is 90μm and 160μm respectively. Through electron microscope magnification 100 times, it is observed that the glass glaze layer is completely integrated with the resistor body, such as Figures 2-3 As shown in the figure, when the thickness of the glaze layer reaches more than 270μm, the glaze layer will begin to sag and the appearance will deteriorate, but the insulation performance will not be affected.
[0082] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a side insulating coating of a ZnO varistor sheet, comprising the following steps: A) Preheating the ZnO varistor to 80-150°C, then spraying the environmentally friendly lead-free glass glaze paint on the side of the ZnO varistor, using the temperature of the preheated ZnO varistor itself to dry the side paint without sagging, to obtain a paint layer; The environmentally friendly lead-free glass enamel coating comprises the following components in percentage by mass: PEG20000: 2%~3.5%, lead-free glass powder: 65%~75%, ethanol: 18%~25%, water: 10%~15%; The lead-free glass powder comprises the following components by mass fraction: bismuth: 74±5.0%, silicon: 3.7±0.5%, boron: 2.8±0.3%, zinc: 11.6±1.0%, aluminum: 2.60±0.3%, lithium: 0.8±0.1%, copper: 4.5±0.6%; The value of the spray weight of the environmentally friendly lead-free glass glaze coating is the side area of the ZnO varistor sheet × the empirical coefficient, the spray weight is in g, the side area of the ZnO varistor sheet is in cm 2 The empirical coefficient is 0.085; The thickness of the insulating coating on the side of the ZnO varistor sheet is 150 to 250 μm; B) subjecting the coating layer to a vitrification heat treatment, heating the coating layer from room temperature to 350° C. at a rate of 1 to 2.5° C. / min, maintaining the temperature at 350° C. for 2 hours, performing binder removal, and after the temperature maintenance, heating the coating layer to 450 to 550° C. at a rate of 1.0 to 1.5° C. / min and maintaining the temperature for 1 hour to obtain a side insulating coating of the ZnO varistor sheet.
2. The preparation method according to claim 1, characterized in that: The spraying in step A) is electrostatic spraying or slurry spraying.
3. The preparation method according to claim 1, characterized in that: The environmentally friendly lead-free glass glaze coating is prepared according to the following steps: PEG20000, water and ethanol are mixed, and then lead-free glass powder is added, and the mixture is evenly stirred and ball-milled for 2 to 6 hours to obtain an environmentally friendly lead-free glass glaze coating.
4. The insulating coating on the side of a ZnO varistor sheet prepared by the preparation method according to any one of claims 1 to 3.
Citation Information
Patent Citations
Heat-dissipation coating with phase-changing temperature adjusting function and preparing method of heat-dissipation coating
CN107337985A
Preparation method of water-based glass glaze and resistor disc
CN111517648A
Method for uniformly refining low-temperature lead-free glass powder by using ultrahigh-pressure microjet and application thereof
CN113149445A
Preparation method of low-melting-point sealing glass powder for micro electronic mechanical system
CN115286253A
Glass sealing material, electrical penetration assembly and preparation method
CN116062997A