A stain-resistant and easy-to-clean UV varnish for automobile interior and a preparation method thereof
By using stain-resistant monomer resin in automotive interior coatings and combining the polymerization technology of UV photoinitiator, a stain-resistant and easy-to-clean UV varnish is prepared, which solves the problem of easy and difficult to keep dirt on the surface of automotive interiors, and achieves a good Cleanliness and durability.
Patent Information
- Application Number
- CN202310740244.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-21
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-06-21
AI Technical Summary
The surface of existing automotive interior paints is prone to dirt after treatment, making it difficult to clean.
Ester solvents, photoinitiators, nine-functional silicone acrylic resins, difunctional agglomerated polyurethane acrylic resins, tetrafunctional agglomerated polyester acrylic resins, pentafunctional agglomerated polyurethane acrylic resins, trifunctional monomer resins, stain-resistant monomer resins, fluorine-based agglomerated Components such as agents and silicone additives are dispersed by dispersing the disperser to prepare stain-resistant and easy-to-clean UV varnish, and polymerized under the action of a photoinitiator to form a stain-resistant monomer resin with hydrophobic properties.
This stain-resistant and easy-to-clean UV varnish makes stains not easy to adhere to the surface of the car interior, and the adhered stains are easy to wipe and remove, significantly improving the cleanliness.
Smart Images

Figure BDA0004297070440000051 
Figure BDA0004297070440000061
Abstract
Description
Technical Field
[0001] The invention relates to the field of automobile varnish, and in particular to a stain-resistant and easy-to-clean UV varnish for automobile interior decoration and a preparation method thereof. Background Art
[0002] With the development of the times, cars play an increasingly important role in people's daily lives, becoming people's second home. Therefore, people's requirements for cars are getting higher and higher, especially in the coatings used for automotive interior parts. In addition to the traditional decorative and aesthetic requirements, they must also be comfortable and durable, which can not only help people relieve fatigue and improve the comfort of use, but also extend the service life of interior parts.
[0003] However, the surface of automobile interiors treated with existing interior paints is prone to dirt and is difficult to clean. Summary of the invention
[0004] In order to overcome the above technical problems, the purpose of the present invention is to provide a stain-resistant and easy-to-clean UV varnish for automobile interior and a preparation method thereof: by adding an ester solvent into a container, turning on a disperser, adding a photoinitiator for dispersion, then adding a nine-functional silicone acrylic resin, a two-functional polyurethane acrylic resin, a four-functional polyester acrylic resin, a five-functional polyurethane acrylic resin, a trifunctional monomer resin, and a stain-resistant monomer resin into the container for continued dispersion, then adding a fluorine auxiliary agent, a silicone auxiliary agent, a ketone solvent, and an alcohol solvent into the container for continued dispersion, to obtain the stain-resistant and easy-to-clean UV varnish for automobile interior, which solves the problem that the surface of the automobile interior treated with the existing interior paint is easy to leave dirt and difficult to clean.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A method for preparing a stain-resistant and easy-to-clean UV varnish for automobile interior, comprising the following steps:
[0007] Step 1: Add the ester solvent into the container, turn on the disperser, adjust the speed to 300-500r / min, add the photoinitiator and disperse for 5-10 minutes;
[0008] Step 2: Add nine-functional silicone acrylic resin, two-functional polyurethane acrylic resin, four-functional polyester acrylic resin, five-functional polyurethane acrylic resin, three-functional monomer resin, and stain-resistant monomer resin into a container, adjust the speed to 600-800r / min and continue to disperse for 25-30min;
[0009] Step 3: Add fluorine additives, silicone additives, ketone solvents, and alcohol solvents into a container and continue to disperse for 25-30 minutes to obtain the stain-resistant and easy-to-clean UV varnish for automotive interior.
[0010] As a further solution of the present invention: the stain-resistant and easy-to-clean UV varnish for automobile interior is used for spraying automobile interior.
[0011] As a further solution of the present invention: the humidity condition during the construction of the stain-resistant and easy-to-clean UV varnish for automobile interior is 50-70%.
[0012] As a further solution of the present invention: the temperature condition during the construction of the stain-resistant and easy-to-clean UV varnish for automobile interior is 5-25°C.
[0013] As a further solution of the present invention: the film thickness of the stain-resistant and easy-to-clean UV varnish for automobile interior is 18-30 um.
[0014] As a further solution of the present invention: the stain-resistant monomer resin is prepared by the following steps:
[0015] Step a1: add alanine, anhydrous potassium carbonate and anhydrous ethanol to a four-necked flask equipped with a stirrer, a thermometer, a constant pressure dropping funnel and a reflux condenser, stir and react for 20-30 minutes at a temperature of 25-30°C and a stirring rate of 300-400r / min, then add allyl chloride dropwise while stirring, and control the dropping rate to 1-2 drops / s. After the dropwise addition is completed, the temperature is raised to reflux and the stirring reaction is continued for 3-5 hours. After the reaction is completed, the reaction product is cooled to room temperature, and then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain intermediate 1;
[0016] Step a2: Add intermediate 1, thionyl chloride and dichloromethane to a three-necked flask equipped with a stirrer and a thermometer, stir and react for 30-40 minutes at a temperature of 0-5°C and a stirring rate of 300-400 r / min, then heat to 40-45°C and continue stirring and reacting for 10-15 hours. After the reaction is completed, cool the reaction product to room temperature, and then remove the solvent by rotary evaporation to obtain intermediate 2;
[0017] Step a3: Add intermediate 2, perfluorodecanol, anhydrous potassium carbonate, p-benzoquinone and N,N-dimethylformamide into a three-necked flask equipped with a stirrer, a thermometer, an air duct and a reflux condenser, introduce nitrogen protection, stir the reaction at a temperature of 25-30°C and a stirring rate of 300-400r / min for 1-1.5h, then raise the temperature to reflux and continue stirring the reaction for 8-10h. After the reaction is completed, the reaction product is cooled to room temperature, and then the solvent is removed by rotary evaporation, and then recrystallized with ethyl acetate to obtain a stain-resistant monomer resin.
[0018] As a further solution of the present invention: the usage ratio of alanine, anhydrous potassium carbonate, anhydrous ethanol and allyl chloride in step a1 is 0.1 mol: 0.11-0.13 mol: 80-100 mL: 0.1 mol.
[0019] As a further solution of the present invention: the usage ratio of the intermediate 1, thionyl chloride and dichloromethane in step a2 is 0.1 mol: 0.12-0.13 mol: 100-120 mL.
[0020] As a further scheme of the present invention: the usage ratio of the intermediate 2, perfluorodecanol, anhydrous potassium carbonate, p-benzoquinone and N,N-dimethylformamide in step a3 is 10mmol:10mmol:12-15mmol:0.02-0.05g:50-60mL.
[0021] As a further solution of the present invention: a stain-resistant and easy-to-clean UV varnish for automobile interior, comprising the following components in parts by weight:
[0022] 20-25 parts of nine-functional silicone acrylic resin, 20-25 parts of difunctional polyurethane acrylic resin, 8-10 parts of tetrafunctional polyester acrylic resin, 10-15 parts of pentafunctional polyurethane acrylic resin, 15-20 parts of trifunctional monomer resin, 1-11 parts of stain-resistant monomer resin, 0.3-0.5 parts of fluorine additives, 0.3-0.5 parts of silicone additives, 3-5 parts of photoinitiator, 5-8 parts of ketone solvents, 10-15 parts of ester solvents, and 5-8 parts of alcohol solvents.
[0023] Beneficial effects of the present invention:
[0024] The invention discloses a stain-resistant and easy-to-clean UV varnish for automobile interior and a preparation method thereof. The method comprises the following steps: adding an ester solvent into a container, turning on a disperser, adding a photoinitiator for dispersion, then adding a nine-functional silicone acrylic resin, a two-functional polyurethane acrylic resin, a four-functional polyester acrylic resin, a five-functional polyurethane acrylic resin, a three-functional monomer resin, and a stain-resistant monomer resin into the container for further dispersion, then adding a fluorine auxiliary agent, a silicone auxiliary agent, a ketone solvent, and an alcohol solvent into the container for further dispersion, thereby obtaining the stain-resistant and easy-to-clean UV varnish for automobile interior. In the process of preparing the stain-resistant and easy-to-clean UV varnish, a stain-resistant monomer resin is firstly prepared, and a nucleophilic substitution reaction is carried out between the amino group on alanine and the chlorine atom on the allyl chloride to introduce the stain-resistant monomer resin. The invention relates to an alkene group and a carboxyl group to obtain an intermediate 1, and then the carboxyl group on the intermediate 1 is chlorinated by using thionyl chloride to introduce an acyl chloride group and enhance the reaction activity to obtain an intermediate 2, and then the acyl chloride group on the intermediate 2 reacts with the hydroxyl group on the perfluorodecyl alcohol to undergo a nucleophilic substitution reaction to obtain a stain-resistant monomer resin; the stain-resistant monomer resin contains an alkene group and a large number of CF bonds on the molecular chain, and the presence of the alkene group enables it to be polymerized with other resin monomers under the action of a photoinitiator, and the introduced CF bonds have low surface energy, giving it good hydrophobic and oleophobic properties, so that stains are not easy to adhere and are easy to wipe and remove after adhesion. Therefore, after the stain-resistant monomer resin is added to the stain-resistant and easy-to-clean UV varnish, it can be sprayed on the interior of the car, so that the interior of the car is not stained with adhesion and is easy to clean. DETAILED DESCRIPTION
[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] Embodiment 1:
[0027] This embodiment is a method for preparing a stain-resistant monomer resin, comprising the following steps:
[0028] Step a1: 0.1 mol of alanine, 0.11 mol of anhydrous potassium carbonate and 80 mL of anhydrous ethanol were added to a four-necked flask equipped with a stirrer, a thermometer, a constant pressure dropping funnel and a reflux condenser, and stirred for reaction at a temperature of 25° C. and a stirring rate of 300 r / min for 20 min, and then 0.1 mol of allyl chloride was added dropwise while stirring, and the dropping rate was controlled to be 1 drop / s. After the addition was completed, the temperature was raised to reflux and the stirring reaction was continued for 3 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered, and the filtrate was rotary evaporated to remove the solvent to obtain intermediate 1;
[0029] Step a2: 0.1 mol of intermediate 1, 0.12 mol of thionyl chloride and 100 mL of dichloromethane were added to a three-necked flask equipped with a stirrer and a thermometer, and stirred for reaction at 0°C and a stirring rate of 300 r / min for 30 min, then heated to 40°C and continued to stir for 10 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain intermediate 2;
[0030] Step a3: Add 10 mmol of intermediate 2, 10 mmol of perfluorodecanol, 12 mmol of anhydrous potassium carbonate, 0.02 g of p-benzoquinone and 50 mL of N,N-dimethylformamide into a three-necked flask equipped with a stirrer, a thermometer, an air duct and a reflux condenser, introduce nitrogen protection, stir the reaction at a temperature of 25°C and a stirring rate of 300 r / min for 1 hour, then raise the temperature to reflux and continue stirring the reaction for 8 hours. After the reaction is completed, the reaction product is cooled to room temperature, then rotary evaporated to remove the solvent, and then recrystallized with ethyl acetate to obtain a stain-resistant monomer resin.
[0031] Embodiment 2:
[0032] This embodiment is a method for preparing a stain-resistant monomer resin, comprising the following steps:
[0033] Step a1: 0.1 mol of alanine, 0.13 mol of anhydrous potassium carbonate and 100 mL of anhydrous ethanol were added to a four-necked flask equipped with a stirrer, a thermometer, a constant pressure dropping funnel and a reflux condenser, and stirred for reaction at a temperature of 30° C. and a stirring rate of 400 r / min for 30 min, and then 0.1 mol of allyl chloride was added dropwise while stirring, and the dropping rate was controlled to be 2 drops / s. After the addition was completed, the temperature was raised to reflux and the stirring reaction was continued for 5 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered, and the filtrate was rotary evaporated to remove the solvent to obtain intermediate 1;
[0034] Step a2: 0.1 mol of intermediate 1, 0.13 mol of thionyl chloride and 120 mL of dichloromethane were added to a three-necked flask equipped with a stirrer and a thermometer, and stirred for reaction at 5°C and a stirring rate of 400 r / min for 40 min, then heated to 45°C and continued to stir for 15 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain intermediate 2;
[0035] Step a3: Add 10 mmol of intermediate 2, 10 mmol of perfluorodecanol, 15 mmol of anhydrous potassium carbonate, 0.05 g of p-benzoquinone and 60 mL of N,N-dimethylformamide into a three-necked flask equipped with a stirrer, a thermometer, an air duct and a reflux condenser, introduce nitrogen protection, stir the reaction at a temperature of 30°C and a stirring rate of 400 r / min for 1.5 hours, then raise the temperature to reflux and continue stirring the reaction for 10 hours. After the reaction is completed, the reaction product is cooled to room temperature, then rotary evaporated to remove the solvent, and then recrystallized with ethyl acetate to obtain a stain-resistant monomer resin.
[0036] Embodiment 3:
[0037] This embodiment is a method for preparing a stain-resistant and easy-to-clean UV varnish for automobile interior, comprising the following steps:
[0038] Step 1: Weigh 20 parts of nine-functional silicone acrylic resin, 20 parts of difunctional polyurethane acrylic resin, 8 parts of four-functional polyester acrylic resin, 10 parts of five-functional polyurethane acrylic resin, 15 parts of trifunctional monomer resin, 1 part of stain-resistant monomer resin from Example 1, 0.3 parts of fluorine additives, 0.3 parts of silicone additives, 3 parts of photoinitiator, 5 parts of ketone solvents, 10 parts of ester solvents, and 5 parts of alcohol solvents according to weight parts, and set aside;
[0039] Step 2: Add the ester solvent into the container, turn on the disperser, adjust the speed to 300r / min, add the photoinitiator and disperse for 5 minutes;
[0040] Step 3: Add nine-functional silicone acrylic resin, two-functional polyurethane acrylic resin, four-functional polyester acrylic resin, five-functional polyurethane acrylic resin, three-functional monomer resin, and stain-resistant monomer resin into a container, and continue to disperse for 25 minutes under the condition of adjusting the speed to 600r / min;
[0041] Step 4: Add fluorine additives, silicone additives, ketone solvents, and alcohol solvents into a container and continue to disperse for 25 minutes to obtain the stain-resistant and easy-to-clean UV varnish for automotive interior.
[0042] Embodiment 4:
[0043] This embodiment is a method for preparing a stain-resistant and easy-to-clean UV varnish for automobile interior, comprising the following steps:
[0044] Step 1: Weigh 25 parts of nine-functional silicone acrylic resin, 25 parts of two-functional polyurethane acrylic resin, 10 parts of four-functional polyester acrylic resin, 15 parts of five-functional polyurethane acrylic resin, 20 parts of trifunctional monomer resin, 11 parts of stain-resistant monomer resin from Example 2, 0.5 parts of fluorine additives, 0.5 parts of silicone additives, 5 parts of photoinitiator, 8 parts of ketone solvent, 15 parts of ester solvent, and 8 parts of alcohol solvent according to weight parts, and set aside;
[0045] Step 2: Add the ester solvent into the container, turn on the disperser, adjust the speed to 500r / min, add the photoinitiator and disperse for 10 minutes;
[0046] Step 3: Add nine-functional silicone acrylic resin, two-functional polyurethane acrylic resin, four-functional polyester acrylic resin, five-functional polyurethane acrylic resin, three-functional monomer resin, and stain-resistant monomer resin into a container, and continue to disperse for 30 minutes under the condition of adjusting the speed to 800r / min;
[0047] Step 4: Add fluorine additives, silicone additives, ketone solvents, and alcohol solvents into a container and continue to disperse for 30 minutes to obtain the stain-resistant and easy-to-clean UV varnish for automotive interior.
[0048] The automobile interior of Example 4 was tested with a stain-resistant and easy-to-clean UV varnish, and the test results are shown in the following table:
[0049]
[0050] Comparative Example 1:
[0051] The difference between Comparative Example 1 and Example 4 is that no stain-resistant monomer resin is added.
[0052] Comparative Example 2:
[0053] The stain-resistant and easy-to-clean UV varnish for automobile interior of Comparative Example 2 comprises the components in parts by weight as shown in the following table:
[0054] Hexafunctional acrylic resin 20-25 servings Difunctional polyurethane acrylic resin 20-25 servings Tetrafunctional polyester acrylic resin 8-10 servings Pentafunctional polyurethane acrylic resin 10-15 servings Trifunctional monomer resin 15-20 servings Fluorine additives 0.3-0.5 parts Silicone additives 0.3-0.5 parts Photoinitiator 3-5 servings Ketone solvents 5-8 servings Ester solvents 10-15 servings Alcohol solvents 5-8 servings
[0055] Comparative Example 3:
[0056] The stain-resistant and easy-to-clean UV varnish for automobile interior of Comparative Example 3 comprises the components in parts by weight as shown in the following table:
[0057] Silicone hydroxy acrylic resin 65-70 servings Polyester acrylic resin 10-20 servings Ketone solvents 15-20 servings Silicone leveling agent 0.2 parts Acrylic leveling agent 0.3 parts Ester solvents 10-15 servings
[0058] The stain-resistant and easy-to-clean UV varnish for automobile interior of Examples 3-4 and Comparative Examples 1-3 was tested, and the test results are as follows:
[0059]
[0060] Referring to the data in the above table, it can be known that the stain-resistant and easy-to-clean UV varnish for automobile interior of the present invention has better stain resistance and is easier to clean.
[0061] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0062] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A method for preparing a stain-resistant and easy-to-clean UV varnish for automobile interior, characterized in that: The following steps are involved: Step 1: weigh 20-25 parts of nine-functional silicone acrylic resin, 20-25 parts of two-functional polyurethane acrylic resin, 8-10 parts of four-functional polyester acrylic resin, 10-15 parts of five-functional polyurethane acrylic resin, 15-20 parts of trifunctional monomer resin, 1-11 parts of stain-resistant monomer resin, 0.3-0.5 parts of fluorine additives, 0.3-0.5 parts of silicone additives, 3-5 parts of photoinitiator, 5-8 parts of ketone solvent, 10-15 parts of ester solvent, 5-8 parts of alcohol solvent according to weight parts, and set aside; Step 2: Add the ester solvent into the container, turn on the disperser, adjust the speed to 300-500r / min, add the photoinitiator and disperse for 5-10 minutes; Step 3: Add nine-functional silicone acrylic resin, two-functional polyurethane acrylic resin, four-functional polyester acrylic resin, five-functional polyurethane acrylic resin, three-functional monomer resin, and stain-resistant monomer resin into a container, adjust the speed to 600-800r / min and continue to disperse for 25-30min; Step 4: adding fluorine additives, silicone additives, ketone solvents, and alcohol solvents into a container and continuing to disperse for 25-30 minutes to obtain the stain-resistant and easy-to-clean UV varnish for automotive interior decoration; The stain-resistant monomer resin is prepared by the following steps: Step a1: add alanine, anhydrous potassium carbonate and anhydrous ethanol to a four-necked flask equipped with a stirrer, a thermometer, a constant pressure dropping funnel and a reflux condenser, stir and react for 20-30 minutes at a temperature of 25-30°C and a stirring rate of 300-400r / min, then add allyl chloride dropwise while stirring, and control the dropping rate to 1-2 drops / s. After the dropwise addition is completed, the temperature is raised to reflux and the stirring reaction is continued for 3-5 hours. After the reaction is completed, the reaction product is cooled to room temperature, and then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain intermediate 1; the amount ratio of alanine, anhydrous potassium carbonate, anhydrous ethanol and allyl chloride in step a1 is 0.1mol: 0.11-0.13mol: 80-100mL: 0.1mol; Step a2: adding intermediate 1, thionyl chloride and dichloromethane to a three-necked flask equipped with a stirrer and a thermometer, stirring the mixture for 30-40 min at a temperature of 0-5° C. and a stirring rate of 300-400 r / min, then heating the mixture to 40-45° C. and continuing to stir the mixture for 10-15 h. After the reaction is completed, cooling the reaction product to room temperature, and then removing the solvent by rotary evaporation to obtain intermediate 2; the dosage ratio of intermediate 1, thionyl chloride and dichloromethane in step a2 is 0.1 mol: 0.12-0.13 mol: 100-120 mL; Step a3: Add intermediate 2, perfluorodecanol, anhydrous potassium carbonate, p-benzoquinone and N,N-dimethylformamide to a three-necked flask equipped with a stirrer, a thermometer, an air duct and a reflux condenser, introduce nitrogen protection, stir and react for 1-1.5 hours at a temperature of 25-30°C and a stirring rate of 300-400r / min, then heat to reflux and continue stirring and reacting for 8-10 hours. After the reaction is completed, cool the reaction product to room temperature, then rotary evaporate to remove the solvent, and then recrystallize with ethyl acetate to obtain a stain-resistant monomer resin; the amount ratio of the intermediate 2, perfluorodecanol, anhydrous potassium carbonate, p-benzoquinone and N,N-dimethylformamide in step a3 is 10mmol:10mmol:12-15mmol:0.02-0.05g:50-60mL.
2. The method for preparing a stain-resistant and easy-to-clean UV varnish for automobile interior according to claim 1, characterized in that: The stain-resistant and easy-to-clean UV varnish for automobile interior is used for spraying automobile interior.
3. The method for preparing a stain-resistant and easy-to-clean UV varnish for automobile interior according to claim 1, characterized in that: The humidity condition during the construction of the stain-resistant and easy-to-clean UV varnish for automobile interior is 50-70%.
4. The method for preparing a stain-resistant and easy-to-clean UV varnish for automobile interior according to claim 1, characterized in that: The temperature condition during the construction of the stain-resistant and easy-to-clean UV varnish for automobile interior is 5-25°C.
5. The method for preparing a stain-resistant and easy-to-clean UV varnish for automobile interior according to claim 1, characterized in that: The film thickness of the stain-resistant and easy-to-clean UV varnish for automobile interior is 18-30 um.
6. A stain-resistant and easy-to-clean UV varnish for automobile interior prepared by the method for preparing a stain-resistant and easy-to-clean UV varnish for automobile interior according to any one of claims 1 to 5, characterized in that: It comprises the following components in parts by weight: 20-25 parts of nine-functional silicone acrylic resin, 20-25 parts of difunctional polyurethane acrylic resin, 8-10 parts of tetrafunctional polyester acrylic resin, 10-15 parts of pentafunctional polyurethane acrylic resin, 15-20 parts of trifunctional monomer resin, 1-11 parts of stain-resistant monomer resin, 0.3-0.5 parts of fluorine additives, 0.3-0.5 parts of silicone additives, 3-5 parts of photoinitiator, 5-8 parts of ketone solvents, 10-15 parts of ester solvents, and 5-8 parts of alcohol solvents.