A heat treatment process for optimizing comprehensive mechanical properties of high-temperature titanium alloys manufactured by laser additive manufacturing

Through the triple heat treatment process, the microstructure of the titanium alloy manufactured by laser additive manufacturing is controlled, solving the problem of difficulty in matching its strength and plasticity, and achieving good room temperature and high temperature mechanical properties, which is suitable for the manufacturing needs of complex structural parts.

CN116875925BActive Publication Date: 2024-10-15NORTHEASTERN UNIV CHINA +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310918174.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-25
Publication Date
2024-10-15
Estimated Expiration
2043-07-25

AI Technical Summary

Technical Problem

The microstructure of laser additively manufactured titanium alloys is different from traditional casting and forging. The existing heat treatment process cannot effectively optimize its comprehensive mechanical properties at high temperature and room temperature, resulting in difficulty in matching strength and plasticity.

Method used

A triple heat treatment process is used to evolve the fine needle-like lamellar structure of high-temperature titanium alloy manufactured by laser additive into a composite structure of primary coarse lamella α, fine secondary lamella α and residual β phase. By controlling the heat treatment temperature and time , regulate the microstructure to improve strength and plasticity matching.

Benefits of technology

It achieves good room-temperature strong plasticity matching and better high-temperature tensile and durable properties of laser additively manufactured titanium alloys, meeting the application requirements for high comprehensive performance. The process operation is simple and energy consumption is low, making it suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116875925B_ABST
    Figure CN116875925B_ABST
Patent Text Reader

Abstract

The present invention discloses a heat treatment process for optimizing the comprehensive mechanical properties of laser additively manufactured high-temperature titanium alloys. The process performs triple heat treatment on laser additively manufactured high-temperature titanium alloys to obtain laser additively manufactured titanium alloys with good room temperature strength-plasticity matching and better high temperature tensile and durability performance. The present invention uses triple heat treatment to evolve the fine needle-like lamellar structure of laser additively manufactured titanium alloys into a composite structure with primary coarse lamellar α, fine secondary lamellar α and residual β phase, so that the laser additively manufactured titanium alloy breaks through the limitation that strength and plasticity are difficult to match well, and obtains good room temperature strength-plasticity matching and better high temperature tensile and durability performance to meet the application requirements of high comprehensive performance. The process is simple, the operation is convenient, the processing cycle is short, the energy consumption is low, and it is suitable for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of optimizing comprehensive performance of titanium alloys, and specifically relates to a heat treatment process for optimizing comprehensive mechanical properties of high-temperature titanium alloys manufactured by laser additive manufacturing. Background Art

[0002] Titanium alloys are widely used in aerospace and other fields due to their advantages such as high specific strength, corrosion resistance and good high temperature performance.

[0003] Laser additive manufacturing technology uses high-power melting and synchronous powder delivery to form parts layer by layer. It has the advantages of moldlessness, short cycle, digitalization, and the ability to prepare complex structural parts. This makes it an important path to achieve the integrated structural and functional manufacturing of complex structural parts such as aircraft engines and gas turbines.

[0004] Due to the characteristics of rapid heating and rapid cooling in the laser deposition process, the structure obtained by laser additive manufacturing of titanium alloys is usually a chaotic needle-shaped Widmanstatten structure. In addition, the laser additive manufacturing alloy is no longer subjected to subsequent forging, rolling and other deformations. Therefore, the solidification and heat treatment structure of the laser additive manufacturing titanium alloy is completely different from the traditional casting and forging structure. The heat treatment process for traditional casting and forging titanium alloys will not be suitable for laser additive manufacturing of titanium alloys.

[0005] At present, there have been a lot of research on the heat treatment process for improving the strength-plasticity matching of laser additively manufactured titanium alloys, but there are few reports on the heat treatment process for optimizing the comprehensive mechanical properties of laser additively manufactured titanium alloys at room temperature and high temperature. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a heat treatment process for optimizing the comprehensive mechanical properties of laser additively manufactured high-temperature titanium alloys in view of the deficiencies of the above-mentioned prior art. The process uses triple heat treatment to transform the fine needle-like lamellar structure of laser additively manufactured high-temperature titanium alloys into a composite structure with primary coarse lamellar α, fine secondary lamellar α and residual β phase, so that laser additively manufactured high-temperature titanium alloys break through the limitation of difficult good matching of strength and plasticity, and obtain good room temperature strength and plasticity matching and better high-temperature tensile and endurance performance to meet the application requirements of high comprehensive performance.

[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is: a heat treatment process for optimizing the comprehensive mechanical properties of laser additively manufactured high-temperature titanium alloy, characterized in that the laser additively manufactured high-temperature titanium alloy is subjected to triple heat treatment, so that the laser additively manufactured high-temperature titanium alloy obtains excellent comprehensive mechanical properties with a room temperature yield strength of 1007MPa to 1015MPa, an elongation of 8.3% to 9.5%, a high temperature yield strength of 221MPa to 233MPa at 600℃, and a durability time of 11h to 12.3h at 600℃ / 310MPa.

[0008] The above-mentioned heat treatment process for optimizing the comprehensive mechanical properties of laser additively manufactured high-temperature titanium alloy is characterized in that the laser additively manufactured high-temperature titanium alloy is an α+β type titanium alloy.

[0009] The above-mentioned heat treatment process for optimizing the comprehensive mechanical properties of laser additively manufactured high-temperature titanium alloy is characterized in that the initial structure of the laser additively manufactured high-temperature titanium alloy is a fine needle-like lamellar structure.

[0010] The above-mentioned heat treatment process for optimizing the comprehensive mechanical properties of high-temperature titanium alloys manufactured by laser additive manufacturing is characterized in that the process parameters of the triple heat treatment are: the first heat treatment temperature is T β -(5~10)℃, holding time is 2h~3h, air cooling; the second heat treatment temperature is T β -(20~30)℃, holding time is 2h~3h, air cooling; the third heat treatment temperature is 700℃, holding time is 6h~8h, air cooling, T β It is the β phase transformation temperature of laser additive manufacturing high temperature titanium alloy, in °C.

[0011] The above-mentioned heat treatment process for optimizing the comprehensive mechanical properties of laser additively manufactured high-temperature titanium alloy is characterized in that the laser additively manufactured high-temperature titanium alloy after triple heat treatment has a composite structure of coarse primary lamellar α, fine secondary lamellar α and residual β phase.

[0012] Compared with the prior art, the present invention has the following advantages:

[0013] 1. The present invention uses triple heat treatment to evolve the fine needle-like lamellar structure of laser additively manufactured high-temperature titanium alloy into a composite structure with primary coarse lamellar α, fine secondary lamellar α and residual β phase, so that laser additively manufactured titanium alloy breaks through the limitation that strength and plasticity are difficult to match well, and obtains good room temperature strength and plasticity matching and better high-temperature tensile and endurance performance to meet the required application requirements of high comprehensive performance.

[0014] 2. The present invention selects an α+β type laser additive manufacturing titanium alloy whose initial structure is a fine needle-like lamellar structure. The fine lamellar layers in the initial structure are very easy to ablate or coarsen and grow during the heat treatment process, providing a basis for the subsequent regulation of the content and size of the primary α phase, thereby achieving the purpose of regulating the strength and plasticity of the laser additive manufacturing titanium alloy.

[0015] 3. The present invention controls the first heat treatment temperature to be T β -(5~10)℃, so that the grain boundary α phase in the initial microstructure prepared by laser deposition in the titanium alloy undergoes Oswald ripening at high temperature, making it discontinuous at the grain boundary, thereby improving the strength-plasticity matching of the titanium alloy; then, by controlling the second heat treatment temperature to T β -(20~30)℃, so that the primary coarse lamellar α phase with a volume fraction of 15%~25% is precipitated in the titanium alloy after the first heat treatment, so that it can simultaneously meet the room temperature strength-plasticity matching, good high temperature strength and high temperature long-lasting comprehensive mechanical properties; and then the third heat treatment temperature is controlled to 700℃, which is higher than the high temperature service temperature of the titanium alloy, which plays a role in stabilizing the organization and ensuring its thermal stability, and avoids the excessively high temperature causing the secondary α phase to grow and resulting in a decrease in the yield strength of the titanium alloy.

[0016] 4. The present invention comprehensively considers the effects of changes in parameters such as heat treatment temperature, time, and cooling method on the alloy structure and properties, and effectively regulates the content and size of coarse primary α phase, fine secondary α phase, and residual β phase in the microstructure of laser additively manufactured titanium alloy, so that the laser additively manufactured titanium alloy can achieve a good match between strength and plasticity, and obtain a good room temperature strength-plasticity match and better high-temperature tensile and endurance properties.

[0017] 5. The heat treatment process of the present invention is easy to operate, has a short treatment cycle, and low energy consumption, and is suitable for industrial production.

[0018] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 1 and 2 are initial microstructure diagrams of TC4-DT titanium alloy manufactured by laser additive manufacturing in Example 1 of the present invention and Comparative Example 1.

[0020] Figure 2 This is the microstructure diagram of the TC4-DT titanium alloy made by laser additive manufacturing after the first heat treatment in Example 1 of the present invention.

[0021] Figure 3 This is the microstructure diagram of the TC4-DT titanium alloy after the second heat treatment manufactured by laser additive manufacturing in Example 1 of the present invention.

[0022] Figure 4This is a microstructure diagram of the TC4-DT titanium alloy manufactured by laser additive manufacturing after simple heat treatment in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0023] Example 1

[0024] The specific process of this embodiment is: the laser additively manufactured TC4-DT titanium alloy with fine needle-like lamellar structure is subjected to triple heat treatment: the first heat treatment temperature is 975°C, the holding time is 2 hours, and air cooling; the second heat treatment temperature is 940°C, the holding time is 2 hours, and air cooling; the third heat treatment temperature is 700°C, the holding time is 8 hours, and air cooling to room temperature.

[0025] Figure 1 This is the initial microstructure diagram of the TC4-DT titanium alloy manufactured by laser additive manufacturing in this embodiment. Figure 2 This is the microstructure diagram of the laser additively manufactured TC4-DT titanium alloy after the first heat treatment in this embodiment. Figure 3 This is the microstructure diagram of the laser additively manufactured TC4-DT titanium alloy after the second heat treatment in this embodiment. Figure 1 and Figure 2 It can be seen that after the first heat treatment, the grain boundary α phase in the initial microstructure of the laser additively manufactured TC4-DT titanium alloy melted and broke into discontinuous nearly equiaxed α phase. Figure 3 It can be seen that the microstructure of the laser additively manufactured TC4-DT titanium alloy after the second heat treatment presents a composite structure containing primary coarse α phase layers and fine secondary α phase layers distributed between them.

[0026] After testing, the room temperature yield strength of the laser additively manufactured TC4-DT titanium alloy in this embodiment after triple heat treatment is 1007MPa, the elongation is 9.5%, the 600℃ high temperature tensile yield strength is 221MPa, and the endurance time at 600℃ / 310MPa is 11h, indicating that the titanium alloy has high room temperature strength, good plasticity, and better high temperature tensile and endurance properties.

[0027] Comparative Example 1

[0028] The specific process of this comparative example is: a simple heat treatment is performed on the laser additively manufactured TC4-DT titanium alloy with fine needle-like lamellar structure, which is kept at 700°C for 8 hours and then air-cooled to room temperature.

[0029] Figure 1 This is the initial microstructure of the TC4-DT titanium alloy manufactured by laser additive manufacturing in this comparative example. Figure 4 This is the microstructure of the TC4-DT titanium alloy manufactured by laser additive manufacturing in this comparative example after simple heat treatment. Figure 1 and Figure 4It can be seen that the microstructure of the laser additively manufactured TC4-DT titanium alloy did not change after simple heat treatment, and it was still a basketweave structure with coarse lamellar α phase and residual β phase structure.

[0030] After testing, the room temperature yield strength of the laser additively manufactured TC4-DT titanium alloy in this comparative example after simple heat treatment is 1890MPa, the elongation is 13%, the high temperature tensile yield strength at 700℃ is 199MPa, and the endurance time at 600℃ / 310MPa is 8.5h.

[0031] Combining Example 1 with Comparative Example 1 Figure 1 to Figure 4 By comparison, it can be seen that the present invention evolves the fine needle-like lamellar structure of the laser additively manufactured titanium alloy into a composite structure with primary coarse lamellar α, fine secondary lamellar α and residual β phase through triple heat treatment, thereby enabling the laser additively manufactured titanium alloy to break through the limitation that it is difficult to match strength and plasticity well, and obtain good room temperature strength and plasticity matching and better high temperature tensile and durability.

[0032] Example 2

[0033] The specific process of this embodiment is: the laser additively manufactured TC4-DT titanium alloy with fine needle-like lamellar structure is subjected to triple heat treatment: the first heat treatment temperature is 975°C, the holding time is 3 hours, and air cooling; the second heat treatment temperature is 950°C, the holding time is 3 hours, and air cooling; the third heat treatment temperature is 700°C, the holding time is 6 hours, and air cooling to room temperature.

[0034] According to the detection, the microstructure of the laser additively manufactured TC4-DT titanium alloy after triple heat treatment in this embodiment contains a composite structure in which fine secondary α phase layers are distributed between primary coarse α phase layers.

[0035] After testing, the room temperature yield strength of the laser additively manufactured TC4-DT titanium alloy in this embodiment after triple heat treatment is 1009 MPa, the elongation is 9%, the 600°C high temperature tensile yield strength is 223 MPa, and the endurance time at 600°C / 310 MPa is 11.3 h, indicating that the titanium alloy has high room temperature strength, good plasticity, and better high temperature tensile and endurance properties.

[0036] Example 3

[0037] The specific process of this embodiment is: the laser additively manufactured TC11 titanium alloy with fine needle-like lamellar structure is subjected to triple heat treatment: the first heat treatment temperature is 1007°C, the holding time is 2.5 hours, and air cooling; the second heat treatment temperature is 975°C, the holding time is 2 hours, and air cooling; the third heat treatment temperature is 700°C, the holding time is 7 hours, and air cooling to room temperature.

[0038] According to the detection, the microstructure of the laser additively manufactured TC11 titanium alloy after triple heat treatment in this embodiment contains a composite structure in which fine secondary α phase layers are distributed between primary coarse α phase layers.

[0039] After testing, the room temperature yield strength of the laser additively manufactured TC11 titanium alloy in this embodiment after triple heat treatment is 1013 MPa, the elongation is 8.7%, the 600°C high temperature tensile yield strength is 230 MPa, and the endurance time at 600°C / 310 MPa is 12 hours, indicating that the titanium alloy has high room temperature strength, good plasticity, and better high temperature tensile and endurance properties.

[0040] Example 4

[0041] The specific process of this embodiment is: the laser additively manufactured TC11 titanium alloy with fine needle-like lamellar structure is subjected to triple heat treatment: the first heat treatment temperature is 1015°C, the holding time is 2h, and air cooling; the second heat treatment temperature is 975°C, the holding time is 2.5h, and air cooling; the third heat treatment temperature is 700°C, the holding time is 7h, and air cooling to room temperature.

[0042] According to the detection, the fiber structure of the TC11 titanium alloy manufactured by laser additive manufacturing after triple heat treatment in this embodiment contains a composite structure in which fine secondary α phase layers are distributed between primary coarse α phase layers.

[0043] After testing, the room temperature yield strength of the laser additively manufactured TC11 titanium alloy in this embodiment after triple heat treatment is 1015MPa, the elongation is 8.3%, the 600℃ high temperature tensile yield strength is 233MPa, and the endurance time at 600℃ / 310MPa is 12.3h, indicating that the titanium alloy has high room temperature strength, good plasticity, and better high temperature tensile and endurance properties.

[0044] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A heat treatment process for optimizing the comprehensive mechanical properties of high-temperature titanium alloys manufactured by laser additive manufacturing, characterized in that: The laser additive manufacturing high temperature titanium alloy is an α+β type titanium alloy, and the initial structure is a fine needle-like lamellar structure. The laser additive manufacturing high temperature titanium alloy is subjected to triple heat treatment, so that the laser additive manufacturing high temperature titanium alloy has excellent comprehensive mechanical properties with a room temperature yield strength of 1007MPa~1015MPa, an elongation of 8.3%~9.5%, a high temperature yield strength of 221MPa~233MPa at 600℃, and a durability time of 11h~12.3h at 600℃ / 310MPa. The process parameters of the triple heat treatment are: the first heat treatment temperature is T β -(5~10)℃, holding time is 2h~3h, air cooling; the second heat treatment temperature is T β -(20~30)℃, holding time is 2h~3h, air cooling; the third heat treatment temperature is 700℃, holding time is 6h~8h, air cooling, T β is the β phase transformation temperature of the laser additively manufactured high-temperature titanium alloy, in °C; the laser additively manufactured high-temperature titanium alloy after the triple heat treatment has a composite structure of coarse primary lamellar α, fine secondary lamellar α and residual β phase.