A stainless steel driven roller and processing technology

By using protective coatings composed of ceramic powder, modified graphene, etc., the problem of easy wear and corrosion of stainless steel driven rollers in application is solved, its adhesion and corrosion resistance are improved, and its service life is extended.

CN116904091BActive Publication Date: 2024-10-08KUNSHAN FENFA INSULATING MATERIALS
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310881966.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-18
Publication Date
2024-10-08
Estimated Expiration
2043-07-18

AI Technical Summary

Technical Problem

Stainless steel driven rollers are susceptible to wear and corrosion during application. Common protective coatings are prone to cracks after long-term operation due to uneven distribution of metal powder and insufficient bonding force, affecting their protective capabilities and performance.

Method used

A protective coating composed of ceramic powder, modified graphene, titanate coupling agent, polydopamine and resin is used. The resin is used as a film-forming agent and binder to improve the adhesion effect, and through oxygen plasma treatment and silane coupling The coupling agent is used to graft-modify graphene to enhance the toughness and corrosion resistance of the coating.

Benefits of technology

Significantly improves the adhesion, toughness, wear resistance and corrosion resistance of the protective coating, extends the service life of the driven roller, and enhances its performance under high pressure and high temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004345032210000071
    Figure BDA0004345032210000071
  • Figure BDA0004345032210000081
    Figure BDA0004345032210000081
Patent Text Reader

Abstract

The present application relates to the field of transport rollers, and specifically discloses a stainless steel driven roller and a processing technology. The stainless steel driven roller includes a roller, and the surface of the roller is provided with a protective coating, and the protective coating is formed by spraying a protective coating, and the protective coating includes the following components in mass fractions: 70-85 parts of ceramic powder, 2-6 parts of modified graphene, 0.5-2 parts of titanate coupling agent, 1-3 parts of polydopamine, 4-8 parts of resin, and 1-2 parts of solvent; the modified graphene is graphene grafted with polyacrylamide after oxygen plasma treatment; its processing technology is: polishing the outer surface of the driven roller, and then applying the protective coating on the outer surface of the driven roller by dipping, brushing or electrostatic spraying, baking and drying, cooling, and cleaning. The stainless steel driven roller of the present application has the advantages of excellent corrosion resistance, wear resistance and impact resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of transport rollers, and more specifically, to a stainless steel driven roller and a processing technology thereof. Background Art

[0002] The driven roller is a type of transport roller. It is not directly connected to the power source, but moves under the drive of the transmission belt, chain, etc., and plays an intermediate support role in the transmission and conveying system. Stainless steel alloys are widely used in the manufacture of driven rollers due to their good mechanical properties and room temperature corrosion resistance, and give the driven rollers excellent high pressure resistance and mechanical properties.

[0003] When the driven roller is produced, the steel pipe, the axis and the side plate are generally turned separately first, and then the axis and the side plate are welded. After welding, they are tightly matched with the steel pipe to form the driven roller. Then the connection of the driven roller is welded, and after annealing and grinding, it is packaged and shipped.

[0004] Stainless steel driven rollers are susceptible to wear during use and are easily corroded under high temperature conditions. Therefore, before leaving the factory, the surface of the driven roller needs to be coated or electroplated with a protective coating, mainly a zinc alloy layer. However, common protective coatings will crack after long-term operation due to uneven distribution of metal powders and insufficient bonding with the base metal. They are easily peeled off, affecting the protection ability of the driven roller and further affecting the application performance of the driven roller, so there is room for improvement. Summary of the invention

[0005] In order to improve the protection performance of the driven roller, the present application provides a stainless steel driven roller and a processing technology.

[0006] In the first aspect, the present application provides a stainless steel driven roller, which adopts the following technical solution:

[0007] A stainless steel driven roller comprises a roller, wherein a protective coating is provided on the surface of the roller, wherein the protective coating is formed by spraying a protective coating, and the protective coating comprises the following components in parts by weight:

[0008] 70-85 parts of ceramic powder, 2-6 parts of modified graphene, 0.5-2 parts of titanate coupling agent, 1-3 parts of polydopamine, 4-8 parts of resin, and 1-2 parts of solvent;

[0009] The modified graphene is obtained by grafting graphene with polyacrylamide after being treated with oxygen plasma.

[0010] By adopting the above technical solution, resin is used as a film-forming agent and a binder to improve the adhesion effect to the roller. The titanate coupling agent further improves the adhesion effect of the resin to the roller, improves the toughness of the coating, and improves the compatibility of the ceramic powder and the resin, which is beneficial to improve the dispersibility of the ceramic powder and ensure the uniform dispersion of the protective coating. Polydopamine can improve the adhesion to the roller and can also adhere to the surface of modified graphene or ceramic powder, improve the compatibility with the resin, and further promote the bonding force to the roller.

[0011] The modified graphene has high strength and strong corrosion resistance, and can give the protective coating excellent mechanical properties and corrosion resistance. Polyacrylamide is grafted on the graphene, and the graphene improves the heat resistance of polyacrylamide. The long chains of polyacrylamide can be entangled with the long chains of resin molecules and polydopamine molecules to form a network skeleton structure, which greatly enhances the toughness, impact resistance and high pressure resistance of the protective coating, and is beneficial to provide the adhesion of the protective coating to the body.

[0012] Preferably, based on the mass parts of the ceramic powder, the ceramic powder includes 50-65 parts of TiN, 10-15 parts of Co, 8-10 parts of WC, 5-8 parts of Cr, and 8-10 parts of Ni.

[0013] By adopting the above technical solution, Co and Cr are used as bonding phase metals to improve the toughness of the protective coating. TiN, WC and Ni have high hardness and good heat resistance. Various metal powders cooperate with each other to greatly improve the wear resistance of the protective coating.

[0014] Preferably, the method for preparing the modified graphene comprises:

[0015] Surface treating graphene with oxygen plasma to obtain pretreated graphene;

[0016] Dissolving a silane coupling agent in an ethanol solution with a volume fraction of 50% to prepare a silane coupling agent solution with a concentration of 3-8%, immersing the pretreated graphene therein at 45-55° C. for 18-24 hours, filtering, washing, and drying to obtain coupled modified graphene;

[0017] The coupled modified graphene and acrylamide monomer are added into water in a mass ratio of 2:3-5, dispersed evenly, heated to 70-75° C. under nitrogen protection, an initiator is added thereto, reacted for 10-12 hours, separated, and dried to obtain modified graphene.

[0018] By adopting the above technical scheme, the graphene is surface-modified by oxygen plasma, so that the graphene surface carries groups such as hydroxyl, carbonyl, and carboxyl, the silane coupling agent molecules are bonded with the active groups on the graphene surface, and then acrylamide is grafted onto the graphene, and a polymerization reaction occurs under the action of an initiator, so that the graphene surface is grafted with long-chain polyacrylamide molecules;

[0019] By grafting graphene with silane coupling agent and polyacrylamide, the possibility of graphene molecules agglomerating in the protective coating system is reduced, and the dispersion uniformity of graphene is improved. Graphene can fill the gaps in ceramic powders and the fine cracks and pores formed during the resin curing process, blocking the penetration of corrosive small molecules into the protective coating and enhancing the corrosion resistance of the protective coating.

[0020] The long chains of polyacrylamide are grafted and polymerized on the surface of graphene, and can be cross-linked and entangled with the long chains of polydopamine and resin molecules to form a network structure, thereby enhancing the adhesion of the protective coating to the roller and improving the toughness and impact resistance of the coating.

[0021] Preferably, the initiator is ammonium persulfate, and the mass of the initiator is 1-10% of the mass of the acrylamide monomer.

[0022] Preferably, the silane coupling agent is a combination of one or more of γ-methacryloxypropyltrimethoxysilane, γ-glycidyloxypropyltrimethoxysilane, 3-aminopropyltriethoxysilane, and N-β-(aminoethyl)-γ-aminopropylmethyldiethoxysilane.

[0023] Preferably, the oxygen plasma treatment comprises: placing the graphene in an oxygen plasma box for treatment for 5-10 minutes, and the vacuum degree of the oxygen plasma box is 0.3-0.5 mbar.

[0024] By adopting the above technical solution, oxygen plasma treatment can introduce hydroxyl, carbonyl or carboxyl groups into the graphene molecular chain, thereby improving the surface properties of graphene.

[0025] Preferably, the separation step comprises: extracting with ethanol for 18-24 hours.

[0026] By adopting the above technical solution and using anhydrous ethanol for extraction and separation, the polymer physically adsorbed on the surface of the modified graphene can be removed.

[0027] Preferably, the resin is a polyurethane resin and an epoxy resin in a mass ratio of 1:(1.2-1.5).

[0028] By adopting the above technical scheme, the epoxy resin has excellent adhesion to metal rollers and has good heat resistance and corrosion resistance. The polyurethane resin has good heat resistance and aging resistance, strong toughness and wear resistance. The combination of the two can give the protective coating excellent practical performance.

[0029] Preferably, the solvent is anhydrous ethanol.

[0030] Preferably, the method for preparing the protective coating comprises:

[0031] Resin, solvent, titanate coupling agent and polydopamine are mixed according to a proportion, stirred and mixed, modified graphene is added thereto and dispersed evenly, ceramic powder is added thereto, stirred and dispersed, and a protective coating is obtained.

[0032] In a second aspect, the present application provides a processing technology for a stainless steel driven roller, which adopts the following technical solution:

[0033] A processing technology for a stainless steel driven roller comprises the following steps:

[0034] The outer surface of the driven roller is polished, and then the protective coating is applied to the outer surface of the driven roller by dipping, brushing or electrostatic spraying, and then baked and dried, cooled and cleaned.

[0035] By adopting the above technical solution, a processing technology for producing a stainless steel driven roller with a protective coating can be obtained.

[0036] In summary, this application has the following beneficial effects:

[0037] 1. Since the present application uses resin as a film-forming agent and a binder, and cooperates with a titanate coupling agent and polydopamine, the adhesion strength of the protective coating to the roller is improved, and it is beneficial to improve the uniformity of the dispersion of the ceramic powder, and improve the wear resistance and toughness of the protective coating; the modified graphene has high strength and strong corrosion resistance, and can give the protective coating excellent mechanical properties and corrosion resistance. Polyacrylamide is grafted on the graphene, and the graphene improves the heat resistance of polyacrylamide. The long chain of polyacrylamide can be entangled with the long chain of the resin molecule and the long chain of the polydopamine molecule to form a network skeleton structure, which greatly enhances the toughness, impact resistance and high pressure resistance of the protective coating, and is beneficial to provide the adhesion of the protective coating to the body;

[0038] 2. In the present application, it is preferred to treat graphene with oxygen plasma, and then graft-modify the graphene with a silane coupling agent and polyacrylamide, which reduces the possibility of graphene molecules agglomerating in the protective coating system, improves the dispersion uniformity of graphene, and is beneficial to enhancing the corrosion resistance of the protective coating; the long chains of polyacrylamide are grafted and polymerized on the surface of graphene, and can be cross-linked and entangled with the long chains of polydopamine and resin molecules to form a network structure, thereby enhancing the adhesion of the protective coating to the roller and improving the toughness and impact resistance of the coating. DETAILED DESCRIPTION

[0039] The present application is further described in detail below in conjunction with embodiments.

[0040] Preparation Example

[0041] Preparation Example 1

[0042] This preparation example provides a modified graphene, and the preparation method is as follows:

[0043] The graphene was treated in an oxygen plasma box with a vacuum degree of 0.3 mbar for 5 min to obtain pretreated graphene;

[0044] Anhydrous ethanol and water are mixed in a volume ratio of 1:1, a silane coupling agent is dissolved therein, and a silane coupling agent solution with a concentration of 5% is prepared, and the pretreated graphene is immersed in the solution at a bath ratio of 1:10, immersed at 50° C. for 24 hours, filtered, washed, and vacuum dried to obtain coupled modified graphene grafted with coupling agent molecules;

[0045] The coupled modified graphene was immersed in water at a bath ratio of 1:10, acrylamide monomer was added thereto, the mass ratio of coupled modified graphene to acrylamide monomer was 2:3, mixed well, heated to 70° C. under nitrogen protection, and ammonium persulfate was added thereto, the mass of ammonium persulfate being 3% of the acrylamide monomer;

[0046] After reacting for 12 hours, the mixture was extracted with anhydrous ethanol for 12 hours and then dried in vacuum to obtain modified graphene grafted with polyacrylamide.

[0047] In this embodiment, the average particle size of graphene is 4 μm, and the silane coupling agent is KH-570.

[0048] Preparation Example 2

[0049] The only difference between this preparation example and preparation example 1 is that the mass ratio of the coupled modified graphene to the acrylamide monomer is 2:4.

[0050] Preparation Example 3

[0051] The only difference between this preparation example and preparation example 1 is that the mass ratio of the coupled modified graphene to the acrylamide monomer is 2:5.

[0052] Preparation Example 4

[0053] The difference between this preparation example and preparation example 1 is that polyacrylamide is not grafted, the modified graphene is graphene treated with oxygen plasma and modified by silane coupling, and the preparation method is as follows:

[0054] The graphene was treated in an oxygen plasma box with a vacuum degree of 0.3 mbar for 5 min to obtain pretreated graphene;

[0055] Anhydrous ethanol and water are mixed in a volume ratio of 1:1, and a silane coupling agent is dissolved therein to prepare a silane coupling agent solution with a concentration of 5%. The pretreated graphene is immersed in the solution at a bath ratio of 1:10, immersed at 50°C for 24 hours, filtered, washed, and vacuum dried to obtain modified graphene grafted with coupling agent molecules.

[0056] Preparation Example 5

[0057] This preparation example provides a ceramic powder, which is obtained by mixing and ball milling 55 parts of TiN, 13 parts of Co, 10 parts of WC, 6 parts of Cr, and 8 parts of Ni by weight. In this example, the average particle size of the ceramic powder is 80 μm.

[0058] Preparation Example 6

[0059] This preparation example provides a protective coating, including 7.5 kg of ceramic powder, 0.4 kg of modified graphene, 0.1 kg of titanate coupling agent, 0.2 kg of polydopamine, 0.6 kg of resin, and 0.15 kg of solvent.

[0060] In this embodiment, the ceramic powder is the ceramic powder in Preparation Example 5, the modified graphene is prepared by Preparation Example 1, the model of the titanate coupling agent is NXH-201, the resin is a polyurethane resin and a bisphenol A epoxy resin in a mass ratio of 1:1.2; and the solvent is anhydrous ethanol.

[0061] The method for preparing the protective coating comprises:

[0062] The resin, solvent, titanate coupling agent and polydopamine of the above mass are mixed, stirred and mixed, the modified graphene is added thereto, stirred and dispersed, and the ceramic powder is added thereto, stirred and dispersed to obtain a protective coating.

[0063] Preparation Example 7

[0064] The only difference between this preparation example and preparation example 6 is that the protective coating includes the following components in mass: 7 kg ceramic powder, 0.4 kg modified graphene, 0.05 kg titanate coupling agent, 0.2 kg polydopamine, 0.4 kg resin, and 0.1 kg solvent.

[0065] Preparation Example 8

[0066] The only difference between this preparation example and preparation example 6 is that the protective coating includes the following components in mass: 8.5 kg ceramic powder, 0.4 kg modified graphene, 0.2 kg titanate coupling agent, 0.2 kg polydopamine, 0.8 kg resin, and 0.2 kg solvent.

[0067] Preparation Example 9

[0068] The only difference between this preparation example and preparation example 6 is that the modified graphene is 0.2 kg.

[0069] Preparation Example 10

[0070] The only difference between this preparation example and preparation example 6 is that the modified graphene is 0.6 kg.

[0071] Preparation Example 11

[0072] The only difference between this preparation example and preparation example 6 is that no modified graphene is added, that is, the protective coating includes 7.5 kg of ceramic powder, 0.1 kg of titanate coupling agent, 0.2 kg of polydopamine, 0.6 kg of resin, and 0.15 kg of solvent.

[0073] Preparation Example 12

[0074] The only difference between this preparation example and preparation example 6 is that the modified graphene is 0.1 kg.

[0075] Preparation Example 13

[0076] The only difference between this preparation example and preparation example 6 is that the modified graphene is 0.7 kg.

[0077] Preparation Example 14

[0078] The only difference between this preparation example and preparation example 6 is that the modified graphene is prepared by preparation example 2.

[0079] Preparation Example 15

[0080] The only difference between this preparation example and preparation example 6 is that the modified graphene is prepared by preparation example 3.

[0081] Preparation Example 16

[0082] The only difference between this preparation example and preparation example 6 is that the modified graphene is prepared by preparation example 4.

[0083] Preparation Example 17

[0084] The difference between this preparation example and preparation example 6 is that no modified graphene is added, and 0.4 kg of polyacrylamide is added. That is, the protective coating includes 7.5 kg of ceramic powder, 0.4 kg of polyacrylamide, 0.1 kg of titanate coupling agent, 0.2 kg of polydopamine, 0.6 kg of resin, and 0.15 kg of solvent.

[0085] Preparation Example 18

[0086] The only difference between this preparation example and preparation example 6 is that the protective coating includes 7.5 kg of ceramic powder, 0.16 kg of modified graphene prepared in preparation example 4, 0.24 kg of polyacrylamide, 0.1 kg of titanate coupling agent, 0.2 kg of polydopamine, 0.6 kg of resin, and 0.15 kg of solvent.

[0087] Preparation Example 19

[0088] The only difference between this preparation example and preparation example 6 is that the amount of polydopamine is 0.1 kg.

[0089] Preparation Example 20

[0090] The only difference between this preparation example and preparation example 6 is that the amount of polydopamine is 0.3 kg.

[0091] Preparation Example 21

[0092] The only difference between this preparation example and preparation example 6 is that polydopamine is not added. That is, the protective coating includes 7.5 kg of ceramic powder, 0.4 kg of modified graphene, 0.1 kg of titanate coupling agent, 0.6 kg of resin, and 0.15 kg of solvent.

[0093] Example

[0094] Example 1

[0095] A stainless steel driven roller comprises a roller, the surface of which is coated with a protective coating, the thickness of the protective coating being 0.2 mm. The processing technology of the stainless steel driven roller comprises:

[0096] The outer surface of the driven roller is polished, and the protective coating is applied to the outer surface of the driven roller by electrostatic spraying, baked at 220°C for 2 minutes, naturally cooled to room temperature, and cleaned.

[0097] In this example, the protective coating is prepared by Preparation Example 6.

[0098] Embodiment 2-9

[0099] Examples 2-9 are substantially the same as Example 1, except that the protective coatings are prepared from Preparation Examples 7-10, Preparation Example 14, Preparation Example 15, Preparation Example 19, and Preparation Example 20, respectively.

[0100] Comparative Example

[0101] Comparative Example 1

[0102] The only difference between Comparative Example 1 and Example 1 is that the protective coating is prepared by Preparation Example 11.

[0103] Comparative Examples 2-9

[0104] Comparative Examples 2-9 are substantially the same as Comparative Example 1, except that the protective coatings are prepared from Preparation Example 12, Preparation Example 13, Preparation Examples 16-18, and Preparation Example 21, respectively.

[0105] Performance test test 1: neutral salt spray resistance test: test the time required for the driven rollers prepared in each embodiment and comparative example to show white corrosion or blistering in a 4% sodium chloride atmosphere;

[0106] Test 2: Wear test: A falling sand test was carried out with reference to GB5237.4-2008 to detect the wear value of the driven rollers prepared in each embodiment and comparative example;

[0107] Test 3: Impact resistance: The impact resistance test was carried out according to GB / T 1732. After a 1kg hammer was dropped from 50cm, the coating changes were observed and divided into 0-5 levels, where 0 means no cracks and 5 means obvious cracks;

[0108] Test 4: Adhesion: Refer to GB / T 9286, use the cross-cut method to test the adhesion of the coating, and grade it according to the rating standards specified in GB / T9286, where 0 is the best and 5 is poor;

[0109] The results are summarized in Table 1

[0110] Table 1

[0111]

[0112]

[0113] In combination with Examples 1-3 and Table 1, it can be seen that the protective coating prepared according to the method disclosed in the present application can give the driven roller better corrosion resistance, wear resistance and impact resistance, and has good adhesion to the driven roller.

[0114] In combination with Example 1, Example 6, Example 7 and Comparative Example 1, and in combination with Table 1, it can be seen that adding modified graphene can improve the corrosion resistance, wear resistance, impact resistance and adhesion of the protective coating. This may be because graphene can fill the gaps between ceramic powders, improve wear resistance, and can block the penetration of corrosive small molecules, improve corrosion resistance, and the long chains of polyacrylamide can be cross-linked and entangled with the long chains of resin and polydopamine, thereby improving the impact resistance and adhesion of the protective coating. In combination with Example 1, Comparative Examples 4-6 and in combination with Table 1, it can be seen that according to the method disclosed in the present application, the modified graphene obtained by grafting polyacrylamide onto graphene can give the protective coating a more excellent protective performance.

[0115] Combining Example 1, Examples 4-5 and Comparative Examples 2-3 and Table 1, it can be seen that when the amount of modified graphene added is too little, the improvement effect is not obvious. In Example 5, the coating surface is relatively rough, and in Comparative Example 3, the roughness of the coating surface is more obvious. In order to ensure the flatness of the coating surface, the amount of modified graphene added should not be too much. The protective coating is prepared with reference to the formula disclosed in this application, which can ensure that the protective coating has excellent performance while ensuring the surface flatness of the driven roller.

[0116] In combination with Example 1, Examples 8-9, Comparative Example 7 and Table 1, it can be seen that the addition of polydopamine can promote the improvement of the impact resistance and adhesion strength of the coating. This may be because polydopamine participates in the formation of the network skeleton structure of the protective coating, increases the cross-linking degree of the protective coating, is beneficial to improve the adhesion of the protective coating to the roller, and improves the toughness and impact resistance of the protective coating.

[0117] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A stainless steel driven roller, It is characterized in that It comprises a roller, the surface of which is provided with a protective coating, the protective coating being formed by spraying a protective coating, the protective coating comprising the following components in parts by weight: Ceramic powder 70-85 parts, 2-6 parts of modified graphene, Titanate coupling agent 0.5-2 parts, 1-3 parts of polydopamine, Resin 4-8 parts, 1-2 parts of solvent; The modified graphene is obtained by grafting graphene with polyacrylamide after being treated with oxygen plasma; The preparation method of the modified graphene comprises: Surface treating graphene with oxygen plasma to obtain pretreated graphene; The silane coupling agent is dissolved in an ethanol solution with a volume fraction of 50% to prepare a silane coupling agent solution with a concentration of 3-8%, and the pretreated graphene is immersed therein at 45-55° C. for 18-24 hours, filtered, washed, and dried to obtain coupled modified graphene; Add the coupled modified graphene and acrylamide monomer into water in a mass ratio of 2:3-5, disperse them evenly, heat them to 70-75° C. under nitrogen protection, add an initiator, react for 10-12 hours, separate and dry them to obtain modified graphene; The ceramic powder comprises 50-65 parts of TiN, 10-15 parts of Co, 8-10 parts of WC, 5-8 parts of Cr, and 8-10 parts of Ni in parts by mass of the ceramic powder; The resin is a polyurethane resin and an epoxy resin in a mass ratio of 1:(1.2-1.5).

2. The stainless steel driven roller according to claim 1, Features: The initiator is ammonium persulfate, and the mass of the initiator is 1-10% of the mass of the acrylamide monomer.

3. The stainless steel driven roller according to claim 1, Features: The silane coupling agent is a combination of one or more of γ-methacryloxypropyl trimethoxysilane, γ-glycidyloxypropyl trimethoxysilane, 3-aminopropyl triethoxysilane, and N-β-(aminoethyl)-γ-aminopropyl methyl diethoxysilane.

4. The stainless steel driven roller according to claim 1, Features: The oxygen plasma treatment comprises: placing the graphene in an oxygen plasma box for treatment for 5-10 minutes, wherein the vacuum degree of the oxygen plasma box is 0.3-0.5 mbar.

5. The stainless steel driven roller according to claim 1, Features: The separation step comprises: extracting with ethanol for 18-24 hours.

6. The stainless steel driven roller according to claim 1, Features: The preparation method of the protective coating comprises: Resin, solvent, titanate coupling agent and polydopamine are mixed according to a proportion, stirred and mixed, modified graphene is added thereto and dispersed evenly, ceramic powder is added thereto, stirred and dispersed, and a protective coating is obtained.

7. A process for processing a stainless steel driven roller as claimed in any one of claims 1 to 6, Features: The following steps are involved: The outer surface of the driven roller is polished, and then the protective coating is applied to the outer surface of the driven roller by dipping, brushing or electrostatic spraying, and then baked and dried, cooled and cleaned.

Citation Information

Patent Citations

  • Graphene composite powder material and preparation method thereof

    CN104310388A

  • Outer-repairing and inner-curing type graphene functionalization self-repairing microcapsule with cellular structure and preparation method of self-repairing microcapsule

    CN108993330A

  • Ceramic slurry for aluminizing protection and preparation method and application of ceramic slurry

    CN112853350A

  • Titanium carbonitride-based thermal spraying powder and preparation method and application thereof

    CN114000085A

  • Modified graphene anticorrosive paint and preparation method thereof

    CN114921145A