Molds, mold manufacturing methods, extrusion equipment, and pellet manufacturing methods
By setting multiple heat insulation sections inside the mold and rationally configuring the heat source, the problem of molten resin blockage was solved, achieving a balance between mold performance and strength, and improving the quality of the granules and the efficiency of the device.
Patent Information
- Application Number
- CN202180093019.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-03-26
- Filing Date
- 2021-11-01
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2041-11-01
AI Technical Summary
When manufacturing thermoplastic resin granules containing fillers, the molten resin solidifies in the mold nozzle orifice, causing blockage. Furthermore, when an insulation layer is installed inside the mold, it is difficult to balance performance and strength.
Multiple heat insulation sections are set inside the mold, with heat insulation layers extending from the outer periphery to the inner side. Combined with appropriate heat source configuration, the shape and position of the heat insulation layers are optimized to prevent the resin from curing in the nozzle and maintain the mold strength.
It effectively suppresses nozzle clogging, ensures uniform particle size and quality, and improves the performance of the die and extrusion device.
Smart Images

Figure CN116963894B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to molds, methods for manufacturing molds, extrusion apparatus having molds, and methods for manufacturing granules using extrusion apparatus, and is preferably applicable to molds having heat insulation layers. Background Technology
[0002] Previously, when manufacturing granules of thermoplastic resins containing fillers (such as polypropylene (PP) composites), the phenomenon of molten resin solidifying in the nozzle orifice (clogging) when passing through the nozzle orifice set inside the mold became a problem.
[0003] For example, Patent Document 1 discloses a technique of providing an air chamber for heat insulation between the mold surface and the cover plate around a nozzle hole located inside the mold plate body.
[0004] Existing technical documents
[0005] Patent documents
[0006] Patent Document 1: Japanese Patent Application No. 2012-500131 Summary of the Invention
[0007] The problem that the invention aims to solve
[0008] By incorporating a heat insulation layer inside the mold, it is hoped that the phenomenon of resin solidification (clogging) in the nozzle orifice can be suppressed as molten resin passes through the nozzle. However, if the heat insulation layer inside the mold is insufficient, the effect of suppressing resin solidification in the nozzle orifice is minimal. On the other hand, if the heat insulation layer inside the mold is excessive, the mold's strength decreases, potentially leading to related problems. Therefore, it is desirable to balance both mold performance and strength.
[0009] Other topics and new features can be found in the description and figures in this specification.
[0010] Methods for solving problems
[0011] One embodiment of the mold includes: a first component comprising a first metallic material; an injection hole formed from a surface of the first component into the interior of the first component; a plurality of nozzles formed from a surface opposite to the first component into the interior of the first component and connected to the injection hole; a heat source disposed within the first component; and a plurality of first heat insulation portions disposed within the first component. The plurality of first heat insulation portions, when viewed in plan view, extend from the outer periphery of the first component toward the inner side of the first component.
[0012] The effects of the invention
[0013] According to one embodiment, the performance of the mold and the extrusion device equipped with the mold can be improved. Furthermore, the quality of the manufactured granules can be improved using the extrusion device. Attached Figure Description
[0014] Figure 1 This is a schematic diagram illustrating an extrusion apparatus in one embodiment.
[0015] Figure 2 This is a plan view showing a mold in one embodiment.
[0016] Figure 3 This is a plan perspective view showing a mold in one embodiment.
[0017] Figure 4 This is a plan perspective view showing a mold in one embodiment.
[0018] Figure 5 This is a cross-sectional view showing a mold in one embodiment.
[0019] Figure 6 It is Figure 3 A magnified view of a portion of the image.
[0020] Figure 7 This is a cross-sectional view showing a mold in one embodiment.
[0021] Figure 8 It is Figure 7 A magnified view of a portion of the image. Detailed Implementation
[0022] Hereinafter, embodiments will be described in detail based on the accompanying drawings. It should be noted that throughout all the drawings used to describe the embodiments, components with the same function are labeled with the same reference numerals, and repeated descriptions are omitted. Furthermore, in the following embodiments, unless specifically required, identical or similar parts will generally not be described repeatedly.
[0023] In addition, in the drawings used in the embodiments, in order to make the drawings clear and easy to understand, sometimes even sectional views omit section lines, and sometimes even plan views are labeled with section lines.
[0024] (Implementation Method)
[0025] <Example of Extrusion Device Configuration>
[0026] Figure 1 This is a schematic diagram showing the extrusion apparatus (extruder) 1 in this embodiment. It should be noted that... Figure 1 In the middle, for ease of understanding, the screw 3 built into the cylinder 2 is shown in perspective.
[0027] First, refer to Figure 1 To illustrate the general structure of extrusion device 1. Figure 1 The extrusion apparatus 1 shown includes a cylinder (tube) 2, a screw 3 rotatably (freely) disposed within the cylinder 2, a drive mechanism 4 for rotating the screw 3 within the cylinder 2, a hopper (resin feeding section) 5 disposed on the upstream (rear) side of the cylinder 2, and a die 6 mounted on the front (downstream) end of the cylinder 2. The hopper 5 is connected to the upper surface of the cylinder 2, allowing resin material to be supplied into the cylinder 2 via the hopper 5. The cylinder 2 is temperature-controlled by a temperature adjustment mechanism (temperature regulating mechanism) not shown, such as a heater. The extrusion apparatus 1 may also have a filler supply device (not shown) connected to the cylinder 2, in which case desired filler can be supplied into the cylinder 2 from the filler supply device. Alternatively, the extrusion apparatus 1 may also have an injection nozzle (not shown) connected to the cylinder 2, in which case desired additives, etc., can be supplied into the cylinder 2 from the injection nozzle.
[0028] It should be noted that when referring to the extrusion device 1 as the "downstream side" and the "upstream side", the "downstream side" refers to the downstream side of the resin flow in the extrusion device 1, and the "upstream side" refers to the upstream side of the resin flow in the extrusion device 1. Therefore, in the extrusion device 1, the side closer to the extrusion surface 21b of the die 6 is the downstream side, and the side farther from the extrusion surface 21b of the die 6, that is, the side closer to the hopper 5, is the upstream side.
[0029] Two screws 3 are rotatably (freely) inserted into the interior of the cylinder 2. Therefore, the extrusion device 1 can also be considered a biaxial extrusion device (biaxial extruder). Inside the cylinder 2, the two screws 3 are configured and rotate in an intermeshing manner. The length direction (long side direction, axial direction, extension direction) of the cylinder 2 is the same as the length direction (long side direction, axial direction, extension direction) of the screws inside the cylinder 2.
[0030] It should be noted that in this embodiment, the case where there are two screws 3 inside the cylinder 2 is described. Alternatively, the number of screws 3 inside the cylinder 2 can be set to one. However, when the number of screws 3 inside the cylinder 2 is set to two, the space volume increases. Therefore, with the same screw diameter, the dual-shaft (two screws 3) can improve the raw material supply capacity compared to a single-shaft (one screw 3).
[0031] The die 6 is capable of shaping the molten resin extruded from the cylinder 2 of the extrusion unit 1 into a predetermined cross-sectional shape (here, a rope shape) and discharging it. Therefore, the die 6 is a die for extrusion molding.
[0032] It should be noted that in this application, "melting" is not limited to thermal melting, but also includes dissolving the resin with a solvent or the like. Therefore, not only melting the resin by heating, but also dissolving the resin with a solvent, melting the resin with microwaves, etc., can be included in "molten resin". In addition, liquid resin can also be included in "molten resin".
[0033] The front end (downstream end) of cylinder 2 is connected to mold 6. Mold 6 of extrusion device 1 is mounted on granulator 13, which includes water tank (circulation box) 11 and blade holder 12. Granulator 13 can also be regarded as part of extrusion device 1.
[0034] The mold 6 has surfaces located on opposite sides, namely an injection surface (upstream surface) 21a and an extrusion surface (downstream surface) 21b. The injection surface 21a of the mold 6 is connected to the front end of the cylinder 2, and the extrusion surface 21b of the mold 6 is disposed within a water tank 11. The interior of the water tank 11 is filled with a liquid called particle circulating water (PCW). The liquid constituting the particle circulating water is, for example, water.
[0035] The blade holder 12 is located inside the water tank 11, near the extrusion surface 21b of the mold 6. Multiple blades (cutting blades) are provided on the blade holder 12 in a manner opposite to the extrusion surface 21b of the mold 6. The resin material extruded from the extrusion surface 21b is cut by the blades in the granule circulating water into multiple granules (resin granules) 14.
[0036] <Methods for manufacturing granules>
[0037] Reference Figure 1 This will explain the manufacturing method of the particles.
[0038] In the extrusion apparatus 1, the resin material (thermoplastic resin) supplied from the hopper 5 to the cylinder 2 is melted (i.e., becomes molten resin) while being conveyed forward by the rotation of the screw 3 within the cylinder 2. When filler is supplied into the cylinder 2 from a filler supply device (not shown), the molten resin in the cylinder 2 of the extrusion apparatus 1 becomes filled with filler because the resin (molten resin) and filler are mixed by the rotation of the screw 3.
[0039] In the extrusion apparatus 1, molten resin (resin material) fed forward into the cylinder 2 by the rotation of the screw 3 is extruded from the die 6 mounted at the front end of the cylinder 2. It should be noted that the die 6 has a nozzle 24 for discharging the molten resin, which is extruded (discharged) from the nozzle 24 of the die 6. The die 6 of the extrusion apparatus 1 is connected to a water tank 11, which is filled with granular circulating water. Therefore, the molten resin is extruded from the nozzle 24 of the die 6 into the granular circulating water in the water tank 11. The molten resin (resin material) extruded from the nozzle 24 of the die 6 into the granular circulating water in the water tank 11 is successively cut by a cutter mounted on the cutter holder 12 and cooled and solidified (cured) by the granular circulating water. This forms (molded) granules (resin granules) 14. The granules 14 are then transferred to the outside of the water tank 11. Thus, multiple granules 14 can be obtained using the extrusion apparatus 1 of this embodiment.
[0040] In this embodiment, the case where molten resin (resin material) is extruded from the nozzle 24 of the mold 6 into the water tank 11 (granular circulating water) and cut by a cutter is described. Alternatively, the water tank 11 may be omitted, and the molten resin (resin material) may be extruded from the nozzle 24 of the mold 6 into the air (outside the mold 6) and cut by a cutter.
[0041] <Mold Construction>
[0042] Reference Figures 2-8 The structure of mold 6 in this embodiment will be described. Figure 2 This is a plan view of the mold 6 as seen from the extrusion surface 21b. Figure 2 This is a plan view. To make the attached diagram clear and easy to understand, dotted shading is marked on the rigid plate 6c. Figure 3 and Figure 4 This is a planar perspective view of the mold 6 as seen from the extrusion surface 21b. Figure 3 In the image, the heat insulation layer 31 inside mold 6 is shown with dotted shading. Additionally, in... Figure 4 In the image, the heat source 26 and the heat sensor 27 inside the mold 6 are marked with dotted shadows. Figure 5 This is a cross-sectional view of mold 6. Figures 2-4 The cross-sectional view showing the location of line AA and Figure 5 Roughly corresponding. Figure 6 It is Figure 3 A magnified view of a portion of the image. Figure 7 This is a cross-sectional view of mold 6. Figure 8 It is Figure 7 A partial enlarged view (partial enlarged sectional view) is shown.
[0043] It should be noted that, in the description of the mold 6 structure in this application, "plane" refers to a plane parallel to the extrusion surface 21b or the injection surface 21a, and "plane view" means view from the extrusion surface 21b side or the injection surface 21a side. Furthermore, "section" refers to a plane substantially perpendicular to the extrusion surface 21b or the injection surface 21a, and "section view" means viewing the aforementioned perpendicular plane. Additionally, in this application, for ease of explanation, when viewing in section, the injection surface 21a side is sometimes shown as the lower part and the extrusion surface 21b side as the upper part to describe each configuration.
[0044] In this application, "injection surface 21a" refers to the entire surface of the mold 6 on the side connected to the cylinder 2 (i.e., the upstream side), and "extrusion surface 21b" refers to the entire surface of the mold 6 on the side connected to the water tank 11 (i.e., the downstream side). More specifically, "injection surface 21a" is the surface of the mold 6 with the injection hole 25, and "extrusion surface 21b" is the surface of the mold 6 with the nozzle 24 opening or the surface of the rigid plate 6c with the nozzle 24 opening.
[0045] like Figures 2-8 As shown, mold 6 has a central component 6a and an outer peripheral component 6b surrounding the central component 6a. The outer peripheral component 6b surrounds the central component 6a when viewed in plan view. The central component 6a and the outer peripheral component 6b are independently manufactured parts, but are integrated by joining them together through welding or the like. That is, the outer peripheral component 6b is joined to the central component 6a in a manner that surrounds the central component 6a when viewed in plan view. Furthermore, the central component 6a and the outer peripheral component 6b are each made of a metallic material (e.g., stainless steel), but they can also be made of different materials (different types of stainless steel).
[0046] The mold 6 is provided with connecting holes 22 and 23 for connecting with other components (e.g., cylinder 2). Specifically, a connecting hole 22 is provided in the center of the central component 6a, penetrating the central component 6a, and four connecting holes 23 are provided in the outer peripheral component 6b, penetrating the outer peripheral component 6b. Figure 5 As shown by the dashed line, the mold 6 is connected to the cylinder 2 by setting bolts and other connecting parts 22a and 23a in each connecting hole 22 and 23.
[0047] It should be noted that, on the extrusion surface 21b side, since the cutting tool provided by the tool holder 12 is movable, the peripheral parts of the connecting holes 22 and 23 are formed to be recessed towards the injection surface 21a side compared with other parts, so as to prevent the connecting parts 22a and 23a from protruding from the mold 6 and being cut.
[0048] In addition, the mold 6 also has a hard plate (plate component) 6c, which is disposed on the surface of the central component 6a on the extrusion surface 21b side. The hard plate 6c contains a material with a hardness higher than that of the material constituting the central component 6a (metallic material). That is, the hard plate 6c has a higher hardness than the central component 6a (the metallic material constituting the central component 6a). In addition, the hard plate 6c contains a material with a hardness higher than that of the material constituting the peripheral component 6b (metallic material). The hard plate 6c has, for example, a material containing titanium carbide (TiC) and has a thickness of, for example, 1 to 5 mm. The hard plate 6c and the central component 6a are joined together by brazing, for example, a self-fluxing alloy. This high-hardness hard plate 6c is disposed on the extrusion surface 21b side, thereby suppressing the possibility of the central component 6a being cut by the cutting tool of the tool holder 12.
[0049] Furthermore, multiple nozzles (orifices) 24 are provided on the central component 6a and the rigid plate 6c. Each nozzle 24 has a portion formed on the central component 6a and a portion formed on the rigid plate 6c, and the two portions are connected. That is, the nozzles 24 on the central component 6a and the nozzles 24 on the rigid plate 6c are interconnected, forming an integrated nozzle. Therefore, the nozzles 24 penetrate the rigid plate 6c. In addition, the central component 6a is provided with multiple injection holes 25, and the multiple nozzles 24 are connected (spatially connected) to each injection hole 25. Therefore, the end (upstream end) of each nozzle 24 is connected (connected) to the injection hole 25.
[0050] exist Figures 2-4 In this case, the central component 6a is provided with four injection holes 25. Since each injection hole 25 is connected to 11 nozzles 24, a total of 44 nozzles 24 are provided. It should be noted that the number of nozzles 24 connected to each injection hole 25 is not limited to 11, and can be any number (preferably multiple). In addition, the number of injection holes 25 provided on the central component 6a is preferably four, but can also be any number other than four (single or multiple).
[0051] In the extrusion apparatus 1, molten resin, conveyed forward (downstream) by the rotation of the screw 3 within the cylinder 2, is injected from the cylinder 2 into the mold 6. At this time, the molten resin is injected into the injection hole 25 on the injection surface 21a side. The molten resin injected from the cylinder 2 into the injection hole 25 is extruded from the extrusion surface 21b toward the outside of the mold 6 (specifically, the water tank 11) via the nozzle 24 communicating with the injection hole 25.
[0052] The injection hole 25 is formed from the surface of the injection surface 21a side of the central component 6a into the interior of the central component 6a, has a relatively wide opening area, and is connected to a plurality of nozzles 24.
[0053] The nozzle 24 penetrates the rigid plate 6c, extending from the surface of the extrusion surface 21b of the central component 6a into the interior of the central component 6a, and connects to the injection hole 25. The opening area (opening diameter) of the nozzle 24 is smaller than the opening area of the injection surface 21a.
[0054] In addition, such as Figure 4 and Figure 5 As shown, the mold 6 is provided with multiple heat sources (heaters) 26 mainly used for heating the area around the injection hole 25 and the nozzle 24, and a thermal sensor 27 for measuring the heating temperature of the multiple heat sources 26.
[0055] Each heat source 26 is arranged in a manner that it is not directly connected to the injection hole 25 and the nozzle 24. Therefore, each heat source 26 is positioned in a position that does not overlap with the injection hole 25 and the nozzle 24 when viewed in a planar manner. In addition, if the adjacent heat source 26 clamps the injection hole 25 when viewed in a planar manner, the heat from the heat source 26 can be used to efficiently heat the molten resin passing through the injection hole 25 and the nozzle 24.
[0056] The heat source 26 consists of holes formed on the outer peripheral component 6b and the central component 6a, and a heating mechanism disposed inside the holes. Examples of such a heating mechanism include electric heaters using coils or heat transfer rods, hot oil, or steam. Figure 4 and Figure 5 In this example, heat source 26 is constructed using an electric heater (cylinder heater). When using hot oil or steam as the heating mechanism, for example, a thermal sensor 27 can be used to connect the front ends of two adjacent holes (the holes constituting heat source 26), creating a circulation path. In this case, one hole can be used as an inlet and the other as an outlet. Such connected holes and the hot oil or steam circulating within them can also serve as heat source 26.
[0057] like Figure 3 and Figures 5-8 As shown, the mold 6 is provided with a heat insulation layer (heat insulation part) 31.
[0058] The heat insulation layer 31 is formed by holes provided in the mold 6. That is, the heat insulation layer 31 is formed by cavities (spaces) where there are no metal materials constituting the mold 6. Preferably, the pressure of the gas inside the holes (cavities) constituting the heat insulation layer 31 is atmospheric pressure or a reduced pressure or vacuum lower than atmospheric pressure. It is also possible to make the pressure of the gas inside the holes (cavities) constituting the heat insulation layer 31 greater than atmospheric pressure, but in this case, it is difficult to form the heat insulation layer 31. In addition, when the pressure of the gas inside the holes (cavities) constituting the heat insulation layer 31 is set to reduced pressure or vacuum, the heat insulation effect of the heat insulation layer 31 can be improved compared to the case where it is set to atmospheric pressure.
[0059] A prescribed gas is present (filled) in the holes (cavities) constituting the heat insulation layer 31. The gas in the holes (cavities) constituting the heat insulation layer 31 can be air, nitrogen, or an inactive gas (such as argon). Preferably, the holes (cavities) constituting the heat insulation layer 31 are sealed and not connected to the space outside the mold 6.
[0060] Alternatively, liquid or solid can be filled into the holes (cavities) constituting the heat insulation layer 31 instead of gas. However, compared to filling the holes (cavities) constituting the heat insulation layer 31 with liquid or solid, filling with gas makes it easier to form the heat insulation layer 31 and improves its heat insulation effect, thus it is more preferred. In any case, the heat insulation layer 31 has a lower thermal conductivity than the materials constituting the central component 6a, the outer peripheral component 6b, and the rigid plate 6c. The heat insulation layer 31 has a lower thermal conductivity than the materials surrounding it, thus it can function in a way that does not hinder heat movement (conduction) within the mold 6. In other words, within the mold 6, heat can be suppressed or prevented from moving (conducting) through the heat insulation layer 31.
[0061] The main feature of this embodiment lies in the configuration and shape of the heat insulation layer 31 provided in the mold 6, which will be explained in more detail later. In this embodiment, by studying the configuration and shape of the heat insulation layer 31 provided in the mold 6, the heat insulation effect of the heat insulation layer 31 can be improved, and the reduction in strength of the mold 6 caused by the provision of the heat insulation layer 31 can be suppressed. As a result, the temperature drop and blockage of the resin material can be reliably suppressed or prevented inside the nozzle 24 of the mold 6, and problems that may occur in the event of a reduction in the strength of the mold 6 can be prevented. Therefore, the performance of the mold 6 and the performance of the extrusion device 1 equipped with the mold 6 can be improved. In addition, the quality of the resin product (in this case, granules) manufactured using the extrusion device 1 can be improved.
[0062] <The Research Process>
[0063] As described above, the resin material, after being mixed inside the cylinder 2, is extruded from the extrusion surface 21b (specifically, the nozzle 24) of the mold 6 into the water tank 11, and cut into multiple particles 14 by the cutter provided on the cutter holder 12. At this time, the interior of the water tank 11 is filled with particle circulating water (e.g., water) at a temperature of, for example, around 60°C. The resin material extruded from the nozzle 24 of the mold 6 into the water tank 11 is cooled by the particle circulating water near the extrusion surface 21b and solidifies to a certain degree of hardness or increased viscosity, thus enabling it to be easily cut by the cutter.
[0064] On the other hand, in order to stably extrude resin material from the nozzle 24 of the mold 6 into the water tank 11, the viscosity of the resin material is preferably low to a certain extent inside the injection hole 25 and the nozzle 24 of the mold 6. Therefore, multiple heat sources 26 are provided in the mold 6, and the temperature of each heat source 26 is set to a temperature suitable for the type of resin. The viscosity of the resin material changes corresponding to the temperature of the resin material.
[0065] Here, since the rigid plate 6c is in direct contact with the water tank 11, the cooling effect of the water tank 11 is more significant than the heating effect of the heat source 26 in the region from the surface of the rigid plate 6c to a certain depth. Furthermore, the opening diameter of the nozzle 24 (the opening diameter on the extrusion surface 21b), which roughly determines the size of the particles 14, is very small, for example, about 1 to 4 mm. Therefore, if the resin material cures inside the nozzle 24, it is difficult for the resin material to be extruded from the nozzle 24, resulting in blockage inside the nozzle 24.
[0066] Furthermore, the mold 6 is provided with multiple nozzles 24. If the peripheral temperature of each nozzle 24 is uneven, the degree of clogging in each nozzle 24 is prone to be uneven. There may also be a situation where unclogged nozzles 24 and clogged nozzles 24 are mixed together. As a result, the size of the particles 14 extruded from the nozzles 24 of the mold 6 is uneven, making it difficult to manufacture particles 14 with uniform size. Therefore, it is necessary to suppress or prevent clogging in the nozzles 24 of the mold 6.
[0067] Therefore, within the mold 6, up to the area as close as possible to the water tank 11, the viscosity of the resin material is preferably reduced, and preferably, just before being extruded into the water tank 11, the viscosity of the resin material becomes high enough to be cured or suitable for cutting. For example, within the nozzle 24 of the mold 6, in the area near the injection hole 25, the viscosity of the resin material is preferably low, and in the area near the extrusion surface 21b (i.e., the area near the front end in the nozzle 24), the viscosity of the resin material is preferably high enough to be suitable for cutting or to be cured.
[0068] Therefore, the inventors of this application investigated the case where a heat insulation layer (corresponding to the aforementioned heat insulation layer 31) is provided in the mold 6. By providing a heat insulation layer, the cooling effect of the water tank 11 can be blocked, thus reducing the viscosity of the resin material within the mold 6 up to the area near the water tank 11. When a heat insulation layer is provided in the mold 6, it is desirable to improve the heat insulation effect of the heat insulation layer. The reason for this is that even if a heat insulation layer is provided in the mold 6, if the heat insulation effect of the heat insulation layer is low, it is difficult to reduce the viscosity of the resin material within the mold 6 up to the area near the water tank 11, thus failing to prevent the nozzle 24 from clogging.
[0069] In this way, by providing a heat insulation layer inside the mold 6, it is expected that the phenomenon of resin solidification (clogging) in the nozzle 24 will be suppressed when the molten resin passes through the nozzle 24 inside the mold 6. However, if there is too little heat insulation layer inside the mold 6, the effect of suppressing the phenomenon of resin solidification (clogging) in the nozzle 24 will be smaller. On the other hand, if there is too much heat insulation layer inside the mold 6, the strength of the mold 6 will be reduced, which may cause associated problems.
[0070] <Main Features and Effects>
[0071] The mold 6 includes: a central part 6a; an injection hole 25 formed from the surface of the central part 6a on the side of the injection surface 21a to the interior of the central part 6a; a plurality of nozzles 24 formed from the surface of the central part 6a on the side of the extrusion surface 21b to the interior of the central part 6a and connected to the injection hole 25; a heat source 26 disposed inside the central part 6a; and a heat insulation layer 31 disposed inside the central part 6a.
[0072] The first feature of this embodiment is that the heat insulation layer 31 includes a plurality of heat insulation portions 31a that extend from the outer periphery of the central member 6a toward the inner side of the central member 6a when viewed in plan view. That is, a plurality of heat insulation portions 31a extending from the outer periphery of the central member 6a toward the inner side of the central member 6a when viewed in plan view are provided inside the central member 6a. Specifically, when viewed in plan view, the plurality of heat insulation portions 31a extend radially from the center of the central member 6a toward the outer periphery of the central member 6a. The plurality of heat insulation portions 31a provided inside the central member 6a may also be spatially connected to each other.
[0073] By applying the first feature, multiple heat insulation portions 31a can be efficiently arranged in the central component 6a of the mold 6. Therefore, the total area of the central component 6a of the mold 6 occupied by the heat insulation layer 31 in planar view can be increased, and the heat insulation effect of the heat insulation layer 31 can be improved. Therefore, clogging in each nozzle 24 can be reliably suppressed or prevented.
[0074] Furthermore, by applying the first feature, multiple heat-insulating parts 31a can be arranged uniformly and without deviation in the central component 6a. Therefore, uneven peripheral temperatures are less likely to occur in each nozzle 24, and consequently, uneven clogging is less likely to occur in each nozzle 24. Thus, particles 14 with uniform size can be manufactured.
[0075] Therefore, the performance of the die 6 and the extrusion device 1 equipped with the die 6 can be improved. In addition, the quality of the granules 14 produced using the extrusion device can be improved.
[0076] Furthermore, in the central component 6a of the mold 6, the injection hole 25 is located between the surface of the central component 6a on the injection surface 21a side and the plurality of heat insulation portions 31a. Preferably, the injection hole 25 overlaps with at least a portion of the plurality of heat insulation portions 31a when viewed in plan view. This allows the cooling effect of the water tank 11 to be blocked by the plurality of heat insulation portions 31a, maintaining the temperature of the resin material within the injection hole 25 at an appropriate temperature. Therefore, the viscosity of the resin material within the injection hole 25 can be set to an appropriate viscosity (low viscosity), thereby suppressing or preventing clogging in each nozzle 24.
[0077] Furthermore, in the central component 6a of the mold 6, the heat source 26 is located between the surface of the central component 6a on the injection surface 21a side and the plurality of heat insulation portions 31a. Therefore, in the central component 6a of the mold 6, the heat source 26 can reliably heat the area closer to the injection surface 21a than the plurality of heat insulation portions 31a. Thus, in the central component 6a of the mold 6, the viscosity of the resin material in the area closer to the injection surface 21a than the plurality of heat insulation portions 31a can be set to an appropriate viscosity (low viscosity), thereby suppressing or preventing clogging in each nozzle 24.
[0078] Furthermore, in the central component 6a of the mold 6, multiple nozzles 24 pass between multiple heat insulation portions 31a. From another perspective, in the central component 6a of the mold 6, the multiple heat insulation portions 31a are arranged in a manner that avoids the nozzles 24 and does not overlap with them. Therefore, inside the nozzles 24, in the region closer to the injection surface 21a than the multiple heat insulation portions 31a, the cooling effect of the water tank 11 can be blocked by the heat insulation layer 31, thereby maintaining the temperature of the resin material inside the nozzles 24 at an appropriate temperature. Therefore, in the region closer to the injection surface 21a than the multiple heat insulation portions 31a, the viscosity of the resin material inside the nozzles 24 can be set to an appropriate viscosity (low viscosity), thereby suppressing or preventing clogging in each nozzle 24.
[0079] However, when manufacturing granules 14 using the extrusion device 1, the die 6 generates a load from the extrusion surface 21b side toward the injection surface 21a side. That is, with Figure 7 and Figure 8 The load is generated in the direction of arrow YG shown in the figure. The reason is that the resin material (molten resin) extruded from the nozzle 24 of the die 6 of the extrusion device 1 is cut by the cutter mounted on the cutter holder 12 to produce particles 14. At this time, the cutter is pressed against the extrusion surface 21b of the die 6 while the cutter is rotated. Therefore, the die 6 generates a load associated with pressing the cutter against the extrusion surface 21b side of the die 6, thereby generating a load on the die 6 from the extrusion surface 21b side toward the injection surface 21a side.
[0080] However, while the first feature allows for efficient heat insulation of the heat insulation portion 31a, it also reduces the mechanical strength of the central member 6a. This can cause deformation of the central member 6a when the die 6 applies a load from the extrusion surface 21b towards the injection surface 21a. This is because the heat insulation layer 31, specifically the heat insulation portion 31a, is composed of holes (cavities) in the central member 6a. More specifically, it consists of the holes (cavities) in the central member 6a and the gas present inside them. An increase in the total area of the central member 6a occupied by the heat insulation portion 31a when viewed in plan view leads to a decrease in the mechanical strength of the central member 6a. If the central member 6a deforms due to this decrease in mechanical strength, the quality of the granules 14 produced using the extrusion apparatus may be reduced.
[0081] Therefore, in this embodiment, in order to suppress or prevent a decrease in the mechanical strength of the central component 6a associated with the heat insulation portion 31a, the cross-sectional shape of the heat insulation portion 31a provided in the central component 6a is studied. That is, as a second feature of this embodiment, the cross-sectional shape of each of the plurality of heat insulation portions 31a provided in the central component 6a is such that the interval S1 between adjacent heat insulation portions 31a is (see...). Figure 8 The shape gradually increases as it moves from the extrusion surface 21b side toward the injection surface 21a side. In this case, the interval S1 between adjacent heat insulation portions 31a is larger than the interval S1a near the injection surface 21a side (i.e., S1a < S1b).
[0082] From another perspective, the second feature can also be expressed as follows: That is, the cross-sectional shape of each of the plurality of heat-insulating portions 31a provided in the central component 6a is such that, as the heat-insulating portion 31a approaches the injection surface 21a from the extrusion surface 21b side, the width W1 of the heat-insulating portion 31a increases (see...) Figure 8 The shape gradually decreases in size. In this case, the width W1 of the heat insulation portion 31a is smaller near the injection surface 21a than the width W1a near the extrusion surface 21b (i.e., W1a > W1b). If the width W1 of the heat insulation portion 31a gradually decreases from the extrusion surface 21b side to the injection surface 21a side, then the spacing S1 between adjacent heat insulation portions 31a gradually increases from the extrusion surface 21b side to the injection surface 21a side.
[0083] Here, the interval S1 between adjacent heat insulation portions 31a corresponds to the interval (distance) in a direction substantially perpendicular to the extending direction of the heat insulation portion 31a. Furthermore, the width W1 of the heat insulation portion 31a corresponds to the width (size) in a direction substantially perpendicular to the extending direction of the heat insulation portion 31a. The direction substantially perpendicular to the extending direction of the heat insulation portion 31a is substantially parallel to the thickness direction of the central member 6a. It should be noted that the thickness direction of the central member 6a corresponds to a direction substantially perpendicular to the extrusion surface 21b or the injection surface 21a. Figures 2-4 , Figure 6 and Figure 7 The Z direction shown is the thickness direction of the central component 6a, which is also the thickness direction of the mold 6.
[0084] The spacing S1 between adjacent heat insulation portions 31a corresponds to the width of the metal region between adjacent heat insulation portions 31a. Therefore, as a second feature, the spacing S1 between adjacent heat insulation portions 31a gradually increases as it approaches the injection surface 21a from the extrusion surface 21b side, indicating that the width of the metal region between adjacent heat insulation portions 31a gradually increases as it approaches the injection surface 21a from the extrusion surface 21b side. In the mold 6, when a load is generated from the extrusion surface 21b side toward the injection surface 21a side, this structure (the structure in which the width of the metal region between adjacent heat insulation portions 31a gradually increases as it approaches the injection surface 21a from the extrusion surface 21b side) is suitable for mitigating (dispersing) the concentration of force in the metal region between adjacent heat insulation portions 31a and suppressing the generation of local stress.
[0085] In this embodiment, by applying the second feature, it is possible to suppress or prevent a decrease in the mechanical strength of the central component 6a associated with the heat insulation portion 31a. In the die 6, when a load is generated from the extrusion surface 21b side toward the injection surface 21a side, deformation of the central component 6a can be suppressed or prevented. Therefore, the performance of the die 6 and the extrusion apparatus 1 equipped with the die 6 can be improved. Furthermore, the quality of the granules 14 manufactured using the extrusion apparatus 1 can be improved.
[0086] An example of the dimensions of the heat insulation portion 31a is given below, but it is not limited thereto and can be varied appropriately. The thickness T1 of each heat insulation portion 31a (see...) Figure 8 The width W1 of each heat insulation portion 31a is, for example, about 3 to 7 mm. Furthermore, the width W1 of each heat insulation portion 31a at its maximum position (i.e., the position closest to the extruded surface 21b) is, for example, about 5 to 10 mm. Additionally, the closest distance S2 between adjacent heat insulation portions 31a (corresponding to the interval S1 between the closest portions) is preferably about 0.2 to 5 mm, more preferably about 1 mm. If the closest distance S2 between adjacent heat insulation portions 31a is too small, the strength of the central component 6a decreases; conversely, if the closest distance S2 between adjacent heat insulation portions 31a is too large, the heat insulation effect decreases.
[0087] Furthermore, the cross-sectional shape of the heat insulation portion 31a is such that the width W1 of the heat insulation portion 31a gradually decreases as it moves from the extrusion surface 21b side towards the injection surface 21a side. For example, it can be designed as a semi-circular shape or a semi-elliptical shape with the injection surface 21a side being an arc side (convex side). Figure 8 This situation is illustrated in the image.
[0088] Furthermore, the arrangement of the plurality of heat-insulating parts 31a provided in the central component 6a is described in more detail below. That is, the plurality of heat-insulating parts 31a provided in the central component 6a includes a plurality of heat-insulating parts 31a belonging to group G1 (Group 1), a plurality of heat-insulating parts 31a belonging to group G2 (Group 2), a plurality of heat-insulating parts 31a belonging to group G3 (Group 3), and a plurality of heat-insulating parts 31a belonging to group G4 (Group 4) (see [link to relevant documentation]). Figure 6 ).
[0089] When viewed in plan view, the plurality of heat-insulating portions 31a of group G1 extend along the X direction and are arranged in the Y direction. When viewed in plan view, the plurality of heat-insulating portions 31a of group G2 extend along the Y direction and are arranged in the X direction. When viewed in plan view, the plurality of heat-insulating portions 31a of group G3 extend along the X direction and are arranged in the Y direction, and are located on the opposite side of group G1, separated by the connecting hole 22. When viewed in plan view, the plurality of heat-insulating portions 31a of group G4 extend along the Y direction and are arranged in the X direction, and are located on the opposite side of group G2, separated by the connecting hole 22. Here, the X and Y directions are shown in... Figures 2-4 , Figure 6 and Figure 7 In the middle, the X and Y directions are generally parallel to the extrusion surface 21b or the injection surface 21a, and the X and Y directions are orthogonal to each other. In addition, the Z direction is orthogonal to the X and Y directions, that is, the thickness direction of the central component 6a.
[0090] By arranging the multiple heat insulation parts 31a provided in the central component 6a in such an arrangement, it is possible to configure the multiple heat insulation parts 31a in the central component 6a of the mold 6 more efficiently.
[0091] In this embodiment, in order to further suppress or prevent the reduction of mechanical strength of the central component 6a which is accompanied by the heat insulation part 31a, the arrangement of the multiple heat insulation parts 31a provided in the central component 6a is also studied.
[0092] That is, as a third feature of this embodiment, in each group G1, G2, G3, and G4, when viewed in section (a section view approximately perpendicular to the extension direction of the heat insulation portion 31a), the arrangement of the multiple heat insulation portions 31a is a curved (arched, bow-shaped) arrangement in which the approximate central portion of the arrangement bulges towards the extrusion surface 21b (see...). Figure 7From another perspective, in each group G1, G2, G3, and G4, the distance L1 from the surface of the extruded surface 21b of the central component 6a to each of the multiple heat insulation parts 31a (see...). Figure 7 The distance L1 from the center of the arrangement of the multiple heat insulation portions 31a gradually increases towards both sides. In this case, the distance L1 from the surface of the extrusion surface 21b side of the central member 6a to the heat insulation portion 31a is larger at the positions near the sides of the arrangement of the heat insulation portions 31a than at the position near the center of the arrangement of the heat insulation portions 31a (i.e., L1a < L1b). This arrangement of the multiple heat insulation portions 31a is suitable for mitigating (dispersing) the concentration of force and suppressing the generation of local stress when a load is generated in the mold 6 from the extrusion surface 21b side towards the injection surface 21a side.
[0093] It should be noted that, Figure 7 The cross-sections of the plurality of heat-insulating sections 31a traversing group G4 are shown, corresponding to cross-sections perpendicular to the Z direction and substantially perpendicular to the extending direction (here, the Y direction) of the plurality of heat-insulating sections 31a traversing group G4. The cross-sections of the plurality of heat-insulating sections 31a traversing group G1, group G2, and group G3 are all perpendicular to the Z direction and substantially perpendicular to the extending direction (here, the Y direction) of the plurality of heat-insulating sections 31a traversing group G4. Figure 7 They are largely the same. Additionally, Figure 7 This is a schematic diagram showing the arrangement of the heat insulation part 31a. Therefore, there are cases where other parts besides the heat insulation part (31a) are omitted from the description.
[0094] In this embodiment, by applying the third feature, it is possible to suppress or prevent a decrease in the mechanical strength of the central component 6a associated with the heat insulation portion 31a. When a load is generated in the die 6 from the extrusion surface 21b side toward the injection surface 21a side, deformation of the central component 6a can be suppressed or prevented. Therefore, the performance of the die 6 and the extrusion apparatus 1 equipped with the die 6 can be improved. Furthermore, the quality of the granules 14 produced using the extrusion apparatus 1 can be improved.
[0095] Furthermore, the heat insulation layer 31 further includes a plurality of heat insulation portions 31b extending in the thickness direction (Z direction) of the central component 6a inside the central component 6a. Similar to the heat insulation portions 31a, the heat insulation portions 31b are also composed of holes (cavities) provided in the central component 6a and gas present inside those holes (cavities). The plurality of heat insulation portions 31b provided inside the central component 6a are each connected to the inner end (end near the connecting hole 22) of the plurality of heat insulation portions 31a. Specifically, the inner end of each of the plurality of heat insulation portions 31a is connected (linked) to the end (end near the extrusion surface 21b) of each of the plurality of heat insulation portions 31b. Therefore, each heat insulation portion 31b extends from the end connected to the heat insulation portion 31a toward the injection surface 21a along the thickness direction (Z direction) of the central component 6a. The plurality of heat insulation portions 31b may also be connected by annular heat insulation portions or the like.
[0096] The insulation layer 31 has both an insulation portion 31a and an insulation portion 31b, thereby improving the insulation effect of the insulation layer 31. In addition, by connecting the insulation portion 31a and the insulation portion 31b (spatial connection), it is easy to set the pressure inside the insulation portions 31a and 31b to a reduced pressure or vacuum lower than atmospheric pressure.
[0097] Alternatively, the hole constituting the heat insulation part 31b can also reach the surface of the injection surface 21a side of the central member 6a. In this case, the hole constituting the heat insulation part 31b is preferably blocked (locked) on the surface of the injection surface 21a side of the central member 6a.
[0098] Furthermore, the heat insulation layer 31 further includes a heat insulation portion 31c connected to the outer peripheral end of each heat insulation portion 31a. That is, the inner end of one of the two ends of the heat insulation portion 31a, which is closer to the center of the mold 6 (connecting hole 22), is connected to the heat insulation portion 31b, and the outer peripheral end, which is farther from the center of the mold 6 (connecting hole 22) (in other words, closer to the outer periphery of the mold 6), is connected to the heat insulation portion 31c. Therefore, the heat insulation portion 31a, the heat insulation portion 31b connected to the inner end of the heat insulation portion 31a, and the heat insulation portion 31c connected to the outer peripheral end of the heat insulation portion 31a are spatially connected. When viewed in plan view, the heat insulation portion 31c surrounds multiple heat insulation portions 31a. In the mold 6, the heat insulation portion 31c is provided singly or in multiples. In the mold 6, the heat insulation part 31c can be provided in the central part 6a, the outer peripheral part 6b, or between the side of the central part 6a and the outer peripheral part 6b. The heat insulation part 31c extends from the end connected to the heat insulation part 31a toward the injection surface 21a along the thickness direction (Z direction) of the mold 6.
[0099] The insulation layer 31 has not only an insulation part 31a but also an insulation part 31c, thereby improving the insulation effect of the insulation layer 31. In addition, the insulation parts 31a, 31b and 31c are connected (spatially connected), making it easy to set the pressure inside the insulation parts 31a, 31b and 31c to a reduced pressure or vacuum lower than atmospheric pressure.
[0100] Furthermore, by surrounding the injection hole 25 and the heat source 26 with heat insulation portions 31a, 31b, and 31c, the cooling effect from the water tank 11 is blocked by the heat insulation portions 31a, 31b, and 31c, and the resin material inside the injection hole 25 can be easily controlled to an appropriate temperature using the heat source 26. Therefore, the viscosity of the resin material inside the injection hole 25 can be easily controlled to an appropriate viscosity (low viscosity), thereby more reliably suppressing or preventing clogging in each nozzle 24.
[0101] Furthermore, since the central component 6a experiences loads such as those caused by the cutting tool as described above, it is preferable to use a high-strength metal material. However, metal materials with high strength have low toughness and are prone to cracking. Additionally, the central component 6a experiences thermal expansion due to being heated to a high temperature by the heat source 26. Therefore, in this embodiment, it is preferable that the toughness of the outer peripheral component 6b is higher than that of the central component 6a. That is, it is preferable that the toughness of the metal material constituting the outer peripheral component 6b is higher than that of the metal material constituting the central component 6a. Thus, even if a metal material with lower toughness is chosen for the central component 6a due to prioritizing strength, the outer peripheral component 6b is made of a metal material with high toughness, thereby easily preventing mold 6 from breaking. Furthermore, even if the central component 6a thermally expands due to heating by the heat source 26, this expansion can be absorbed by the high toughness of the outer peripheral component 6b, thus easily preventing mold 6 from breaking. It should be noted that, in terms of toughness, a high elongation in a tensile test or a high impact value in an impact test indicates high toughness.
[0102] <Manufacturing Method of Mold 6>
[0103] The central component 6a of the mold 6 in this embodiment can be manufactured using various methods, and is particularly preferably manufactured using a 3D printer. Examples of manufacturing methods using a 3D printer include, for instance, powder bed fusion lamination, in which powder containing metal material is layered and sintered directly using a high-output laser beam or electron beam; powder bonding lamination, in which binders are added to the powder and fixed using inkjet printing; and thermomelting lamination, in which metal ejected from a nozzle is melted and layered.
[0104] It should be noted that immediately after the central component 6a is manufactured, the heat insulation layer 31, the heat source 26, and the heat sensor 27 are simple holes (spaces) formed inside the central component 6a. However, for ease of understanding, these holes will be described below as the aforementioned configurations.
[0105] Before or after manufacturing the central part 6a using a 3D printer, prepare the outer peripheral part 6b and the rigid plate 6c. The outer peripheral part 6b and the rigid plate 6c are manufactured separately from the central part 6a, but they can also be manufactured using a 3D printer.
[0106] After preparing the central component 6a, the outer peripheral component 6b and the rigid plate 6c, as described above, the central component 6a and the outer peripheral component 6b are joined together, and the central component 6a is surrounded by the outer peripheral component 6b.
[0107] In addition, the central component 6a is connected (joined) to the rigid plate 6c, and the rigid plate 6c is provided on the surface of the central component 6a on the extrusion surface 21b side.
[0108] Thus, mold 6 in this embodiment is manufactured.
[0109] By using a 3D printer to manufacture the central component 6a, a hollow heat insulation layer 31 (heat insulation parts 31a, 31b) can be easily formed inside the central component 6a. In addition, since the central component 6a, including the heat insulation layer 31, is integrally molded, the overall strength of the central component 6a can be improved.
[0110] In particular, when the central component 6a is manufactured using a 3D printer, the aforementioned central component 6a having multiple heat insulation parts 31a can be manufactured easily and reliably.
[0111] The invention proposed by the inventors of this application has been specifically described above based on the embodiments, but the invention is not limited to the foregoing embodiments, and various modifications can be made without departing from its spirit.
[0112] For example, the central component 6a can be formed not only from a single component, but also from multiple components. Furthermore, the outer peripheral component 6b can be formed not only from a single component, but also from multiple components. Additionally, the central component 6a and the outer peripheral component 6b can be formed as separate components, or they can be combined to form a single integrated component.
[0113] Explanation of reference numerals in the attached figures
[0114] 1. Extrusion device
[0115] 2 cylinders
[0116] 3 screws
[0117] 4 Rotary drive mechanism
[0118] 5 hoppers
[0119] 6. Mold
[0120] 6a Central Component
[0121] 6b Outer Peripheral Components
[0122] 6c rigid board
[0123] 11 sink
[0124] 12 Knife Holders
[0125] 13 Granulator
[0126] 14 particles
[0127] 21a Injection Surface
[0128] 21b Extruded surface
[0129] 22, 23 Connecting holes
[0130] 22a and 23a connecting parts
[0131] 24 nozzles
[0132] 25 Injection Hole
[0133] 26 Heat Source
[0134] 27 Thermal Sensor
[0135] 31 Insulation layer
[0136] 31a, 31b, 31c heat insulation sections
[0137] L1 distance
[0138] S1 interval
[0139] W1 width
Claims
1. A mold, characterized in that, It has an extrusion surface and an injection surface located on the opposite side of the extrusion surface. The mold comprises: The first component comprises the first metallic material; An injection hole is formed from the injection surface of the first component to the interior of the first component; Multiple nozzles are formed from the extrusion side surface of the first component to the interior of the first component and connected to the injection port; A heat source is located inside the first component; as well as Multiple first heat insulation sections are disposed inside the first component. The plurality of the first heat insulation portions extend from the outer periphery of the first component toward the inner side of the first component when viewed in plan view. The cross-sectional shape of the plurality of first heat insulation portions is such that the spacing between adjacent first heat insulation portions gradually increases as they move from the extrusion surface side toward the injection surface side.
2. The mold according to claim 1, characterized in that, The plurality of the first heat insulation portions extend radially.
3. The mold according to claim 1, characterized in that, Each of the plurality of the first heat insulation portions includes a hole provided in the first component and gas present inside the hole.
4. The mold according to claim 3, characterized in that, The pressure of the gas inside the orifice is atmospheric pressure or a reduced pressure or vacuum, which is lower than atmospheric pressure.
5. The mold according to claim 1, characterized in that, Each of the plurality of the first heat insulation portions has a cross-sectional shape that gradually decreases in width as it moves from the extrusion surface side toward the injection surface side.
6. The mold according to claim 1, characterized in that, A first connecting hole is provided in the central part of the first component, extending through the first component. The plurality of first heat insulation portions include a plurality of first heat insulation portions belonging to a first group, a plurality of first heat insulation portions belonging to a second group, a plurality of first heat insulation portions belonging to a third group, and a plurality of first heat insulation portions belonging to a fourth group. The plurality of the first heat insulation portions belonging to the first group extend along the first direction when viewed in a plane, and are arranged in a second direction orthogonal to the first direction. The plurality of the first heat insulation portions belonging to the second group extend along the second direction when viewed in a planar view, and are arranged in the first direction. The plurality of the first heat insulation portions belonging to the third group extend along the first direction when viewed in plan view, are arranged in the second direction, and are located on the opposite side of the first group, separated by the first connecting hole. The plurality of the first heat insulation portions belonging to the fourth group extend along the second direction when viewed in a plane, are arranged in the first direction, and are located on the opposite side of the second group through the first connecting hole.
7. The mold according to claim 6, characterized in that, In each of the first, second, third and fourth groups, when viewed in cross-section perpendicular to the extension direction of the plurality of first heat insulation portions, the plurality of first heat insulation portions are arranged in a curved shape that bulges toward the extrusion surface.
8. The mold according to claim 1, characterized in that, It further includes a plurality of second heat insulation portions disposed inside the first component. The plurality of second heat insulation portions are respectively connected to the inner ends of the plurality of first heat insulation portions and extend in the thickness direction of the first component.
9. The mold according to claim 1, characterized in that, The component further includes a plate member disposed on the surface of the first component on the extrusion side, and having a hardness higher than that of the first metal material. The nozzle penetrates the plate component.
10. The mold according to claim 1, characterized in that, It further includes a second component comprising a second metallic material and engaging with the first component in such a way that it surrounds the first component when viewed in the plane.
11. The mold according to claim 10, characterized in that, A third heat insulation part is provided between the first component and the second component. The outer peripheral ends of the plurality of the first heat insulation parts are connected to the third heat insulation part.
12. The mold according to claim 10, characterized in that, The toughness of the second metallic material is higher than that of the first metallic material.
13. The mold according to claim 1, characterized in that, The injection hole is located between the injection surface of the first component and the plurality of first heat insulation portions.
14. The mold according to claim 13, characterized in that, The plurality of nozzles pass between the plurality of the first heat insulation portions.
15. The mold according to claim 1, characterized in that, The heat source is located between the surface of the first component on the injection surface side and the plurality of the first heat insulation parts.
16. An extrusion apparatus, characterized in that, have: The mold as described in claim 1; A cylinder body, with a screw installed inside, and the injection surface of the mold connected to the cylinder body; and A tool holder having a plurality of tools arranged opposite the extrusion surface of the mold.
17. A method for manufacturing particles, characterized in that, Using the extrusion apparatus of claim 16 The method for manufacturing the particles includes the following steps: (a) The process of supplying resin material into the interior of the cylinder; (b) The process of injecting the resin material, after being mixed in the cylinder, into the injection hole of the mold from the injection surface side; (c) The process of extruding the resin material injected into the injection hole from the plurality of nozzles; as well as (d) A process of obtaining multiple particles containing the resin material by cutting the resin material extruded from the nozzle using the cutter. Steps (c) and (d) are performed while the heat source is activated.
18. A method for manufacturing a mold, characterized in that, Includes the following processes: (a) A process of preparing a first component, the first component comprising a first metal material, manufactured using a 3D printer, having an extrusion surface and an injection surface located on the opposite side of the extrusion surface; (b) The process of preparing a second component containing a second metallic material; (c) The process of preparing a plate component, wherein the plate component has a hardness higher than that of the first metal material; (d) A process of joining the second component to the first component in such a way that it surrounds the first component when viewed from a plane viewed from the extruded side; and (e) The process of joining the plate component to the surface of the extruded side of the first component. The first component has: An injection hole is formed from the injection surface of the first component to the interior of the first component; Multiple nozzles are formed from the surface of the first component on the extrusion side to the interior of the first component and are connected to the injection port; A heat source, which is located inside the first component; and Multiple first heat insulation sections are disposed inside the first component. The plurality of the first heat insulation portions extend from the outer periphery of the first component toward the inner side of the first component when viewed in plan view. The cross-sectional shape of the plurality of first heat insulation portions is such that the spacing between adjacent first heat insulation portions gradually increases as they move from the extrusion surface side toward the injection surface side.
19. A mold, characterized in that, It has an extrusion surface and an injection surface located on the opposite side of the extrusion surface. The mold comprises: An injection hole is formed from the injection surface into the interior of the mold; Multiple nozzles are formed from the extrusion surface into the interior of the mold and connected to the injection port; A heat source is located inside the mold. as well as Multiple first heat insulation sections are disposed inside the mold. The plurality of the first heat insulation portions extend from the center of the mold toward the outer periphery when viewed in plan view. The cross-sectional shape of the plurality of first heat insulation portions is such that the spacing between adjacent first heat insulation portions gradually increases as it moves from the extrusion surface side to the injection surface side.
20. The mold according to claim 19, characterized in that, The plurality of the first heat insulation portions extend radially.
21. The mold according to claim 19, characterized in that, Each of the plurality of the first heat insulation portions includes a hole provided in the mold and gas present inside the hole.
22. The mold according to claim 19, characterized in that, Each of the plurality of the first heat insulation portions has a cross-sectional shape that gradually decreases in width as it moves from the extrusion surface side toward the injection surface side.
23. The mold according to claim 19, characterized in that, A first connecting hole is provided in the center of the mold, penetrating the mold. The plurality of first heat insulation portions include a plurality of first heat insulation portions belonging to a first group, a plurality of first heat insulation portions belonging to a second group, a plurality of first heat insulation portions belonging to a third group, and a plurality of first heat insulation portions belonging to a fourth group. The plurality of the first heat insulation portions belonging to the first group extend along the first direction when viewed in a plane, and are arranged in a second direction orthogonal to the first direction. The plurality of the first heat insulation portions belonging to the second group extend along the second direction when viewed in a planar view, and are arranged in the first direction. The plurality of the first heat insulation portions belonging to the third group extend along the first direction when viewed in plan view, are arranged in the second direction, and are located on the opposite side of the first group, separated by the first connecting hole. The plurality of the first heat insulation portions belonging to the fourth group extend along the second direction when viewed in a plane, are arranged in the first direction, and are located on the opposite side of the second group through the first connecting hole.
24. The mold according to claim 23, characterized in that, In each of the first, second, third and fourth groups, when viewed in cross-section perpendicular to the extension direction of the plurality of first heat insulation portions, the plurality of first heat insulation portions are arranged in a curved shape that bulges toward the extrusion surface.
25. The mold according to claim 19, characterized in that, It further includes a plurality of second heat insulation portions disposed inside the mold. The plurality of second heat insulation portions are respectively connected to the inner ends of the plurality of first heat insulation portions and extend in the thickness direction of the mold.
26. The mold according to claim 19, characterized in that, It further includes a third heat insulation portion, which is disposed inside the mold and extends in the thickness direction of the mold. The outer peripheral ends of the plurality of the first heat insulation parts are connected to the third heat insulation part.
Citation Information
Patent Citations
Insulated die plate for underwater particle formation, etc.
JP2012500131A
High open-ratio granulating template with thermal insulating layer
CN101596753A
High hardness 3D printed steel product
CN111386164A
Foamed plastic granulator
CN112536932A
Die for preparing resin pellet