Self-floating heating and heat-insulating mud for rack steel layer casting and preparation and use method thereof
By using self-floating heating insulation mud in the layered casting process of large rack steel ingots, the problems of macrosegregation and shrinkage of the ingots are solved, which significantly improves the composition uniformity and overall quality of the ingots, and reduces production costs. and energy consumption.
Patent Information
- Application Number
- CN202310596322.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-05-25
AI Technical Summary
During the preparation process, large rack steel ingots are prone to macrosegregation, uneven tissue structure and inclusion aggregation, resulting in low material utilization, poor tissue performance of forgings, and traditional overall casting methods cannot effectively avoid solidification defects.
The layered casting process of self-floating heating insulation mud combined with rack steel is adopted. By applying self-floating heating insulation mud to the inner surface of the crucible, layered casting is carried out in the furnace, and bubbles are generated by reacting with the steel. Float and stir the liquid steel to improve the kinetic conditions during the solidification process of the liquid steel.
The macroscopic segregation and shrinkage defects of large rack steel ingots have been significantly improved, the composition uniformity of the ingots has been improved, the overall quality has been improved, the production cycle has been shortened, the production efficiency has been improved, and the production energy consumption and cost have been reduced.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metallurgical casting, and in particular to a self-floating heating and heat-insulating mud for layered casting of rack steel and a preparation and use method thereof. Background Art
[0002] Large rack steel is an important basic material required for high-end equipment in fields such as nuclear power. The heterogeneity problem of large rack steel ingots is a bottleneck restricting the manufacturing, service performance and life of key components of major equipment. Macrosegregation seriously affects the final performance of the ingot.
[0003] For large rack steel, the preparation method currently adopted in my country is to cast the whole piece first and then forge it. Because the ingot of large rack steel is large in size and takes a long time to solidify, and the violent flow of the melt leads to problems such as macro segregation, uneven structure and inclusion aggregation in the preparation process, and the above defects cannot be eliminated through subsequent processing, resulting in low material utilization, substandard forging structure and performance, and even the entire ingot is scrapped. In fact, 60% of the unqualified large rack steel forgings are caused by ingot quality problems. The solidification intrinsic characteristics of large rack steel ingots and the size effect caused by their large size determine that the traditional integral casting method cannot avoid the problem of solidification defects. Therefore, it is urgent to explore a new type of large rack steel ingot preparation technology to solve the contradiction between large-scale and homogenization, and ultimately improve the quality level of large rack steel forgings.
[0004] At present, researchers have tried a variety of casting technologies to improve the macrosegregation problem of large rack steel ingots. Among them, directional solidification technology and electroslag remelting technology can obtain ingots with uniform composition and excellent structure by controlling the solidification direction of the ingot. However, for the production of large rack steel ingots, directional solidification technology cannot effectively control the liquid flow and solidification direction, and the improvement effect on macrosegregation is weak. Electroslag remelting technology has the disadvantages of huge energy consumption and high pollutant emissions.
[0005] 3D printing technology is an emerging rapid prototyping technology with the advantages of simple process, material saving, and wide application range. It can obtain castings with uniform tissue composition. However, this technology will produce defects such as pores and looseness when printing metal materials, and this process cannot be temporarily applied to the preparation of large rack steel ingots.
[0006] The Chinese patent application with publication number CN107335782A discloses "an efficient and clean riser covering agent for ingot casting and its preparation method", which mixes 60% titanium dioxide and 40% aluminum powder to obtain a riser covering agent, which solves the problems of poor working environment and pollution to molten steel of the existing riser covering agent for ingot casting, and prolongs the shrinkage compensation time. However, this method can only be applied to the riser improvement in the casting process of small ingot casting, and it is difficult to affect the internal quality (segregation and shrinkage cavity) of large rack steel ingots.
[0007] The Chinese invention patent with the authorization announcement number CN108889915B discloses "a method for preparing ingots by layer-by-layer pouring based on slag protection", which divides the steel into several portions according to the amount, melts the molten steel one by one, and adds protective slag one by one, and repeats the operation until all the molten steel is poured. The protective slag layer formed by this method floats on the upper surface of the molten steel and can effectively avoid the formation of an oxide layer, but this method has great limitations. The impurities in the protective slag are easily retained in the molten steel and are difficult to float, and the inclusions formed deteriorate the performance of the steel. In addition, it has the disadvantages of complex production process, long process, poor continuous production capacity, etc., and cannot achieve large-scale mass production.
[0008] The Chinese invention patent with the authorization announcement number CN101831579B discloses "a method for preparing a large-sized aluminum alloy ingot", which involves spreading flux on the bottom of a smelting furnace, adding the alloy to the smelting furnace, spreading a covering agent, and smelting and casting to obtain a large-sized aluminum alloy ingot. This method has a certain improvement effect on the defects of the aluminum alloy ingot, but since the heat transfer rate of iron is significantly lower than that of aluminum, it is difficult for this method to improve the internal quality of a large rack steel ingot, and the flux introduces more impurities, making it difficult to use in conjunction with the layered casting process of large rack steel. Summary of the invention
[0009] The present invention provides a self-floating heating and heat-insulating mud for layered casting of rack steel and a preparation and use method thereof. The self-floating heating and heat-insulating mud of the present invention is used in combination with a layered casting process of rack steel, which can significantly improve the macro-segregation and shrinkage defects of large rack steel ingots (hereinafter referred to as ingots), provides a simple, feasible and effective way to improve the degree of homogenization of ingot composition, helps to improve the overall quality of ingots, and also shortens the production cycle, improves production efficiency, thereby increasing ingot production capacity, and reducing production energy consumption and production costs. The present invention is of great significance for breaking through the bottleneck of manufacturing highly homogenized large rack steel ingots, laying a theoretical foundation and industrial application of new technology for casting large rack steel ingots, and improving the manufacturing technology level of key components of large-scale equipment in my country.
[0010] In order to achieve the above object, the present invention adopts the following technical solutions:
[0011] A self-floating heating and heat-insulating mud for rack steel layer casting comprises, by weight percentage, 15% to 20% C, 25% to 50% Fe2O3, 20% to 30% SiO2 and 15% to 25% polyferric sulfate.
[0012] Furthermore, a self-floating heating and heat-insulating mud for layered casting of rack steel comprises, by weight percentage, the following components: C: 18% to 20%, Fe2O3: 35% to 43%, SiO2: 23% to 27%, and polyferric sulfate: 15% to 18%.
[0013] Furthermore, the specific surface area of the self-floating heating and heat-insulating mud is 350±15m 2 / kg, 28-day shrinkage is 0.064% to 0.081%, 28-day wear resistance is 1.81 to 2.27 kg / m 2 The 28-day flexural strength is ≥9.3MPa, and the 28-day compressive strength is 52.8~53.5MPa.
[0014] A method for preparing self-floating heating and heat-insulating mud for rack steel layer casting comprises the following steps:
[0015] a. Mixing: C-containing raw materials, iron oxide, silicon dioxide and polyferric sulfate are crushed and pre-homogenized respectively, and then the pre-homogenized raw materials are mixed, ground and homogenized according to the ratio of self-floating heating and heat-insulating mud;
[0016] b. Drying: Dry the homogenized mixed material at a temperature of 150°C to 250°C for 1 to 3 hours;
[0017] c. Grinding: Cool the dried mixed material and grind it again to obtain the self-floating heating and heat-insulating mud product. When grinding, control the comprehensive moisture content of the grinding mill to less than 1% and the grinding fineness specific surface area to 350±15m 2 / kg.
[0018] Furthermore, in step a, the C-containing raw material is graphite; in terms of mass percentage, the iron oxide is high-purity iron oxide containing more than 99.8% Fe2O3; the silicon dioxide is high-purity silicon dioxide containing more than 99.5% SiO2; and the polyferric sulfate is analytically pure polyferric sulfate with a purity of more than 99.7%.
[0019] Furthermore, in the step a, the crushing particle size is controlled to be ≤50 mm; the grinding fineness is controlled to be 80 um square hole sieve residue percentage <18%; ultrasonic oscillation is used for homogenization, the oscillation frequency is 20 to 30 kHz, and the oscillation time is 15 to 25 hours.
[0020] Furthermore, in the step b, the drying is carried out in a muffle furnace, and the high-temperature mixed material taken out of the muffle furnace is cooled in a grate cooler, and the temperature of the mixed material out of the grate cooler is controlled to be ≤ ambient temperature + 65°C.
[0021] A method for using self-floating heating and heat-insulating mud for rack steel layer casting comprises the following steps:
[0022] a. Before use, fully stir the self-floating heating and insulation mud with pure water and mix them evenly. The mud-water ratio is 1:0.38~1:0.51;
[0023] b. Evenly apply the self-floating heating and heat-insulating mud mixed with water on the inner surface of the crucible, with a thickness of 0.5 to 1.5 cm;
[0024] c. Place the crucible coated with self-floating heating and heat-insulating mud into the furnace and cast it using a layered casting process.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] 1) The self-floating heat-insulating mud and the layered casting process of rack steel (a patent has been applied for in another case on the same day) of the present invention can significantly improve the problems of uneven solidification speed of the riser caused by uneven covering when adding conventional riser covering agents, and significantly improve the macro segregation and shrinkage problems of large rack steel ingots, providing a simple, feasible and effective way to improve the degree of uniformity of the composition of large rack steel ingots;
[0027] 2) It is beneficial to improve the overall quality of large rack steel ingots, shorten the production cycle, improve production efficiency, thereby increasing the production capacity of large rack steel ingots and reducing production energy consumption and production costs;
[0028] 3) The present invention is of great significance for breaking through the bottleneck of manufacturing highly homogenized large rack steel ingots, laying a theoretical foundation and industrial application of new technology for casting large rack steel ingots, and improving the manufacturing technology level of key components of large equipment in my country. DETAILED DESCRIPTION
[0029] The self-floating heating and heat-insulating mud for rack steel layer casting of the present invention comprises, by weight percentage, 15% to 20% C, 25% to 50% Fe2O3, 20% to 30% SiO2 and 15% to 25% polyferric sulfate.
[0030] Furthermore, a self-floating heating and heat-insulating mud for layered casting of rack steel comprises, by weight percentage, the following components: C: 18% to 20%, Fe2O3: 35% to 43%, SiO2: 23% to 27%, and polyferric sulfate: 15% to 18%.
[0031] Furthermore, the specific surface area of the self-floating heating and heat-insulating mud is 350±15m 2 / kg, 28-day shrinkage is 0.064% to 0.081%, 28-day wear resistance is 1.81 to 2.27 kg / m 2 The 28-day flexural strength is ≥9.3MPa, and the 28-day compressive strength is 52.8~53.5MPa.
[0032] A method for preparing self-floating heating and heat-insulating mud for rack steel layer casting comprises the following steps:
[0033] a. Mixing: C-containing raw materials, iron oxide, silicon dioxide and polyferric sulfate are crushed and pre-homogenized respectively, and then the pre-homogenized raw materials are mixed, ground and homogenized according to the ratio of self-floating heating and heat-insulating mud;
[0034] b. Drying: Dry the homogenized mixed material at a temperature of 150°C to 250°C for 1 to 3 hours;
[0035] c. Grinding: Cool the dried mixed material and grind it again to obtain the self-floating heating and heat-insulating mud product. When grinding, control the comprehensive moisture content of the grinding mill to less than 1% and the grinding fineness specific surface area to 350±15m 2 / kg.
[0036] Furthermore, in step a, the C-containing raw material is graphite; in terms of mass percentage, the iron oxide is high-purity iron oxide containing more than 99.8% Fe2O3; the silicon dioxide is high-purity silicon dioxide containing more than 99.5% SiO2; and the polyferric sulfate is analytically pure polyferric sulfate with a purity of more than 99.7%.
[0037] Furthermore, in the step a, the crushing particle size is controlled to be ≤50 mm; the grinding fineness is controlled to be 80 um square hole sieve residue percentage <18%; ultrasonic oscillation is used for homogenization, the oscillation frequency is 20 to 30 kHz, and the oscillation time is 15 to 25 hours.
[0038] Furthermore, in the step b, the drying is carried out in a muffle furnace, and the high-temperature mixed material taken out of the muffle furnace is cooled in a grate cooler, and the temperature of the mixed material out of the grate cooler is controlled to be ≤ ambient temperature + 65°C.
[0039] The method for using the self-floating heating and heat-insulating mud for rack steel layer casting of the present invention comprises the following steps:
[0040] a. Before use, fully stir the self-floating heating and insulation mud with pure water and mix them evenly. The mud-water ratio is 1:0.38~1:0.51;
[0041] b. Evenly apply the self-floating heating and heat-insulating mud mixed with water on the inner surface of the crucible, with a thickness of 0.5 to 1.5 cm;
[0042] c. Place the crucible coated with self-floating heating and heat-insulating mud into the furnace and cast it using a layered casting process.
[0043] The self-floating heat-insulating mud for layered casting described in the present invention contains C, Fe2O3 and SiO2, which react with molten steel to release heat, slow down the cooling rate of the steel, generate bubbles to float and stir the steel, improve the dynamic conditions during the solidification of the steel, significantly improve the looseness and shrinkage during the solidification of the steel, increase the equiaxed crystal ratio of the ingot, refine the grains, and improve the performance of the steel. The added polyferric sulfate, as an inorganic polymer coagulant, can enhance the coagulation degree of various phases in the heat-insulating mud and improve the use effect.
[0044] Large rack steel adopts layered casting process. As the molten steel is cast, the self-floating heat-insulating mud coated on the inner surface of the crucible gradually melts, reacts chemically with the molten steel to produce bubbles, and gradually floats up, stirs the molten steel, gathers and evenly covers the upper surface of the molten steel, slowing down the cooling rate of the molten steel and starting to solidify slowly. After the next layer of molten steel is added, it re-melts and continues to float up along with the self-floating heat-insulating mud on the side wall of the upper crucible, supplementing the central looseness and shrinkage, improving element segregation, improving the dynamic conditions during the solidification of the molten steel, expanding the equiaxed crystal ratio of the ingot, refining the grains, and improving the performance of the steel.
[0045] The self-floating heat-insulating mud of the present invention is used in combination with the layered casting process. According to the test, the internal quality of the steel grade can be effectively improved. The low-multiple rating is improved from level 1 to level 0.5 compared with the conventional process, which is an average improvement of 0.5 levels. The segregation of each element is significantly reduced, and the segregation rate is reduced by more than 20% on average.
[0046] In conventional casting processes, the molten steel is cast in one go, which can easily cause looseness and shrinkage cavities inside the steel, and serious segregation of various elements, which makes it difficult to carry out subsequent forging and other processes. The steel is prone to cracking during use due to insufficient internal quality. The self-floating heating insulation mud described in the present invention is used in conjunction with a layered casting process to significantly improve the macro segregation and shrinkage cavities of large rack steel ingots, providing a simple, feasible and effective way to improve the degree of uniformity of the composition of large rack steel ingots, which helps to improve the overall quality of rack steel ingots, while also shortening the production cycle and improving production efficiency, thereby increasing the production capacity of large rack steel ingots and reducing production energy consumption and production costs.
[0047] The present invention is described in detail below in conjunction with comparative examples and embodiments 1-3, and the advantages and various effects of the present invention will be more clearly presented. It should be understood by those skilled in the art that these specific implementation methods and embodiments are used to illustrate the present invention, rather than to limit the present invention.
[0048] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the following examples can be purchased from the market or prepared by existing methods.
[0049] Four batches of rack steel were smelted in a 500kg vacuum induction furnace as experimental steel. The target composition of the experimental steel is shown in Table 1.
[0050] Table 1 Target composition of rack steel (wt%)
[0051] element C Si Mn Ni Cr Mo Cu V Ti Fe and impurities content 0.33 0.20 0.80 2.70 0.50 0.60 0.40 0.06 0.01 margin
[0052] [Comparative Example]
[0053] The "conventional smelting + conventional casting" process is adopted to cast the rack steel of the first furnace directly after conventional smelting. After the ingot is completely cooled, the longitudinal polishing surface of the wide surface of the ingot is polished to observe the shrinkage cavity distribution, and then the element segregation degree test is carried out.
[0054] [Example 1]
[0055] The rack steel of the second furnace is cast by adopting the process of "conventional smelting + rack steel layered casting" and using the self-floating heating insulation mud of the present invention in combination.
[0056] The specific process is as follows:
[0057] 1. Mixing: crush graphite, high-purity iron oxide with a Fe2O3 content of 99.85%, high-purity silicon dioxide with a SiO2 content of 99.6%, and analytically pure polyferric sulfate with a purity of 99.73% respectively, and pre-homogenize them. Then, according to the ratio of self-floating heating and insulation mud (C: 15%, Fe2O3: 50%, SiO2: 20%, polyferric sulfate: 15%), mix and grind the pre-homogenized raw materials, and homogenize them by ultrasonic vibration, with a vibration frequency of 30kHz and a vibration time of 15h. Control the crushing particle size ≤ 50mm; control the grinding fineness to be less than 18% of the 80um square hole sieve residue;
[0058] 2. Drying: The homogenized mixed material is sent to a muffle furnace for drying at a temperature of 180°C for 2 hours.
[0059] 3. Grinding: Send the dried mixed material to the grate cooler for cooling, and control the temperature of the mixed material out of the grate cooler to be lower than (ambient temperature + 65°C). The cooled mixed material is ground again to obtain self-floating heating and heat-insulating mud. When grinding, control the comprehensive moisture content of the grinding to 0.8%, and the grinding fineness specific surface area to 360m 2 / kg.
[0060] 4. Before using the self-floating heating and insulation mud, add pure water and stir thoroughly to mix evenly. The mud-water ratio is 1:0.38;
[0061] 5. Evenly apply the self-floating heating and heat-insulating mud mixed with water on the inner surface of the crucible with a thickness of 0.5 cm;
[0062] 6. Place the crucible coated with self-floating heating and heat-insulating mud into the furnace and cast it using a layered casting process.
[0063] 7. The self-floating heating and insulation mud melts in the molten steel after being heated, and gradually floats up, evenly covering the top of the riser, isolating the air to play a role in heating and heat preservation, and improving the solidification conditions of the molten steel.
[0064] 8. After the ingot is completely cooled, take the longitudinal polishing surface of the wide surface of the ingot for grinding, observe the shrinkage cavity distribution, and then conduct the element segregation test.
[0065] [Example 2]
[0066] The rack steel of the third furnace is cast by adopting the process of "conventional smelting + rack steel layered casting" and using the self-floating heating insulation mud of the present invention in combination.
[0067] The specific process is as follows:
[0068] 1. Mixing: crush graphite, high-purity iron oxide with a Fe2O3 content of 99.87%, high-purity silicon dioxide with a SiO2 content of 99.7% and analytically pure polyferric sulfate with a purity of 99.75% respectively, and pre-homogenize them. Then, according to the ratio of self-floating heating and insulation mud (C: 20%, Fe2O3: 25%, SiO2: 30%, polyferric sulfate: 25%), mix the pre-homogenized raw materials, grind them, and homogenize them with ultrasonic vibration. The vibration frequency is 20kHz and the vibration time is 25h. Control the crushing particle size ≤50mm; control the grinding fineness to be 80um square hole sieve residue percentage less than 18%;
[0069] 2. Drying: The homogenized mixed material is sent to a muffle furnace for drying at a temperature of 200°C for 3 hours.
[0070] 3. Grinding: Send the dried mixed material to the grate cooler for cooling, and control the temperature of the mixed material out of the grate cooler to be lower than (ambient temperature + 65°C). After cooling, grind again to obtain self-floating heating and heat-insulating mud. When grinding, control the comprehensive moisture content of the grinding to 0.7%, and the grinding fineness specific surface area to 340m 2 / kg.
[0071] 4. Before using the self-floating heating and insulation mud, stir it with pure water and mix it evenly. The mud-water ratio is 1:0.47;
[0072] 5. Evenly apply the self-floating heating and heat-insulating mud mixed with water on the inner surface of the crucible with a thickness of 1.2 cm;
[0073] 6. Place the crucible coated with self-floating heating and heat-insulating mud into the furnace and cast it using a layered casting process.
[0074] 7. The self-floating heating and heat-insulating mud melts in the molten steel under the heat, and gradually floats up, evenly covering the top of the riser, isolating the air to play the role of heating and heat preservation, and improving the solidification conditions of the molten steel.
[0075] 8. After the ingot is completely cooled, take the longitudinal polishing surface of the wide surface of the ingot for grinding, observe the shrinkage cavity distribution, and then conduct the element segregation test.
[0076] [Example 3]
[0077] The rack steel of the fourth furnace is cast by adopting the process of "conventional smelting + rack steel layered casting" and using the self-floating heating insulation mud of the present invention in combination.
[0078] The specific process is as follows:
[0079] 1. Mixing: crush graphite, high-purity iron oxide with a Fe2O3 content of 99.9%, high-purity silicon dioxide with a SiO2 content of 99.6%, and analytically pure polyferric sulfate with a purity of 99.81%, respectively, and pre-homogenize them. Then, according to the ratio of self-floating heating and insulation mud (C: 20%, Fe2O3: 40%, SiO2: 20%, polyferric sulfate: 20%), mix and grind the pre-homogenized raw materials, and homogenize them by ultrasonic vibration. The vibration frequency is 25kHz and the vibration time is 20h. The crushing particle size is ≤50mm; the grinding fineness is controlled to be 80um square hole sieve residue percentage less than 18%;
[0080] 2. Drying: The homogenized mixed material is sent to a muffle furnace for drying at a temperature of 250°C for 1 hour.
[0081] 3. Grinding: Send the dried mixed material to the grate cooler for cooling, and control the temperature of the mixed material out of the grate cooler to be lower than (ambient temperature + 65°C). After cooling, grind again to obtain self-floating heating and heat-insulating mud. When grinding, control the comprehensive moisture content of the grinding to 0.5%, and the grinding fineness specific surface area to 350m 2 / kg.
[0082] 4. Before using the self-floating heating and insulation mud, stir it with pure water and mix it evenly. The mud-water ratio is 1:0.42;
[0083] 5. Evenly apply the self-floating heating and heat-insulating mud mixed with water on the inner surface of the crucible with a thickness of 0.9 cm;
[0084] 6. Place the crucible coated with self-floating heating and heat-insulating mud into the furnace and cast it using a layered casting process;
[0085] 7. The self-floating heating and heat-insulating mud melts into the molten steel under the heat, and gradually floats up, evenly covering the riser, isolating the air to play the role of heating and heat preservation, and improving the solidification conditions of the molten steel;
[0086] 8. After the ingot is completely cooled, take the longitudinal polishing surface of the wide surface of the ingot for grinding, observe the shrinkage cavity distribution, and then conduct the element segregation test.
[0087] The element segregation test results of the comparative example and embodiments 1-3 are shown in Table 2:
[0088] Table 2 Element segregation test results
[0089]
[0090] By comparison, it can be seen that the self-floating heat-insulating mud for layered casting combined with the layered casting process described in the present invention is used. During the casting process, the self-floating heat-insulating mud is heated and melted in the molten steel and gradually floats up, evenly covering the riser, isolating the air to play a role in heating and heat preservation, and improving the solidification conditions of the molten steel. The internal quality of the large rack steel ingots cast in Examples 1-3 is significantly higher than that of the comparative example, which solves the problem of uneven riser solidification speed caused by uneven covering when adding conventional riser covering agents, significantly improves the macro segregation and shrinkage defects of large rack steel ingots, and provides a simple, feasible and effective way to improve the degree of homogenization of the composition of large rack steel ingots, which helps to improve the overall quality of rack steel ingots, and also shortens the production cycle and improves production efficiency, thereby increasing the production capacity of large rack steel ingots and reducing production energy consumption and production costs.
[0091] The above embodiments are only used to illustrate the present invention, and are not used as limitations on the present invention. For example, the iron oxide content, heating temperature, heating time, coating thickness, material particle size, etc. are also limited within the essential scope of the present invention. Changes and modifications to the above embodiments will fall within the scope of protection of the claims of the present invention.
[0092] It should be understood that the endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0093] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A self-floating heating and heat-insulating mud for rack steel layer casting, characterized in that: Used to mix with water and then smeared on the inner surface of the crucible; the self-floating heating and heat-insulating mud includes C: 15% to 20%, Fe2O3: 35% to 50%, SiO2: 20% to 30%, and polyferric sulfate: 15% to 25% by weight; the specific surface area of the self-floating heating and heat-insulating mud is 350±15m 2 / kg, 28-day shrinkage is 0.064% to 0.081%, 28-day wear resistance is 1.81 to 2.27 kg / m 2 The 28-day flexural strength is ≥9.3MPa, and the 28-day compressive strength is 52.8~53.5MPa.
2. The self-floating heating and heat-insulating mud for rack steel layer casting according to claim 1 is characterized in that: The components include, by weight percentage: C: 18%-20%, Fe2O3: 35%-43%, SiO2: 23%-27%, and polyferric sulfate: 15%-18%.
3. The method for preparing the self-floating heating and heat-insulating mud for layered casting of rack steel according to claim 1 or 2, characterized in that: The steps include: a. Mixing: crush the C-containing raw materials, iron oxide, silicon dioxide and polyferric sulfate respectively, and then pre-homogenize them. Then, mix, grind and homogenize the pre-homogenized raw materials according to the ratio of self-floating heating and heat-insulating mud; b. Drying: Dry the homogenized mixed material at a temperature of 150°C to 250°C for 1 to 3 hours; c. Grinding: Cool the dried mixed material and grind it again to obtain the self-floating heating and heat-insulating mud product. When grinding, control the comprehensive moisture content of the grinding mill to less than 1% and the grinding fineness specific surface area to 350±15m 2 / kg.
4. The method for preparing the self-floating heating and heat-insulating mud for rack steel layer casting according to claim 3 is characterized in that: In the step a, the C-containing raw material is graphite; in terms of mass percentage, the iron oxide is high-purity iron oxide containing more than 99.8% of Fe2O3; the silicon dioxide is high-purity silicon dioxide containing more than 99.5% of SiO2; and the polyferric sulfate is analytically pure polyferric sulfate with a purity of more than 99.7%.
5. The method for preparing the self-floating heating and heat-insulating mud for rack steel layer casting according to claim 3, characterized in that: In the step a, the crushing particle size is controlled to be ≤50 mm; the grinding fineness is controlled to be 80 μm square hole sieve residue percentage <18%; ultrasonic oscillation is used for homogenization, the oscillation frequency is 20 to 30 kHz, and the oscillation time is 15 to 25 hours.
6. The method for preparing the self-floating heating and heat-insulating mud for rack steel layer casting according to claim 3, characterized in that: In the step b, the drying is carried out in a muffle furnace, and the high-temperature mixed material taken out of the muffle furnace is cooled in a grate cooler, and the temperature of the mixed material out of the grate cooler is controlled to be ≤ ambient temperature + 65°C.
7. The method for using the self-floating heating and heat-insulating mud for rack steel layer casting as claimed in claim 1 or 2, characterized in that: The steps include: a. Before use, fully stir the self-floating heating and insulation mud with pure water and mix them evenly. The mud-water ratio is 1:0.38~1:0.51; b. Evenly apply the self-floating heating and heat-insulating mud mixed with water on the inner surface of the crucible, with a thickness of 0.5 to 1.5 cm; c. Place the crucible coated with self-floating heating and heat-insulating mud into the furnace and cast it using a layered casting process.
Citation Information
Patent Citations
Preparation method of large-size aluminum alloy ingot
CN101831579B
Efficient and clean riser covering agent for ingot casting and preparation method thereof
CN107335782A
A method for preparing ingots by layer-by-layer casting based on slag protection
CN108889915B
Riser heating and insulating agent
CN101798233A