Anthraquinone compound, liquid crystal composition containing the same and dimming element
By using anthraquinone compounds and photohardening compounds of specific structures in the liquid crystal dimming film, a dimming element with excellent contrast and light resistance is formed, and the problem of insufficient contrast and light resistance in the prior art is solved, and it is suitable for automotive window glasses. and outdoor building materials.
Patent Information
- Application Number
- CN202280019767.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-08
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-03-08
AI Technical Summary
The existing liquid crystal dimming films lack contrast and light resistance during light shading, resulting in high glare and reduced penetration under long-term exposure at high temperatures, making it difficult to meet the transparency and durability requirements of automotive window glass.
Anthraquinone compounds with specific structures are used as dichroic pigments, combined with liquid crystal materials and photohardening compounds, and hardened compounds are formed through photopolymerization initiators to improve the contrast and light resistance of the dimming element.
It realizes dimming elements with excellent contrast and light resistance, ensuring stable penetration under high temperature exposure for a long time, and is suitable for automotive window glass and outdoor building materials.
Smart Images

Figure CN117062877B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a novel anthraquinone compound, a liquid crystal composition containing the compound and a dimming element. Background Art
[0002] For the purpose of protecting privacy, various methods have been proposed for controlling the penetration of external light in windows, doors and partitions of vehicles such as trams and cars, and buildings such as commercial buildings and hospitals (Patent Documents 1 and 2). One of such dimming films uses liquid crystal. Generally, liquid crystal dimming films can control the penetration or scattering of light to block the field of vision by applying voltage or not, but since they cannot block the light itself, there is a tendency for the glare to increase due to light scattering. Therefore, for the purpose of reducing glare or improving contrast, attempts are being made to use pigments in the materials of dimming panels (Patent Documents 3 and 4). When such a dimming panel is used on the window glass of a car, in addition to requiring no turbidity and good vision when transparent, it is also required to obtain a darker color when shading, or light resistance such that the transmittance does not decrease even when exposed to light for a long time at high temperatures due to long-term exposure caused by outdoor use.
[0003] The dye used in the liquid crystal dimming film is generally a dichroic dye. A GH (Guest Host) type dimming element using a liquid crystal composition containing a dichroic dye is known, and various dichroic dyes have been proposed (Patent Documents 5 and 6).
[0004] In such dichroic dyes, in addition to the contrast that is already required in display elements, light resistance and heat resistance are also required. Although efforts have been made to improve these characteristics, no dichroic dye that can meet the contrast and light resistance requirements has been found. For example, Patent Documents 5 and 6 disclose a dichroic dye suitable for dimming purposes, but the contrast and light resistance of the dyes in the same documents are still insufficient.
[0005] [Prior art literature]
[0006] [Patent Document]
[0007] [Patent Document 1] Japanese Patent Publication No. 63-501512
[0008] [Patent Document 2] Japanese Patent Application Laid-Open No. 03-47392
[0009] [Patent Document 3] Japanese Patent Application Publication No. 2018-205746
[0010] [Patent Document 4] Japanese Patent Application Publication No. 2011-190314
[0011] [Patent Document 5] Japanese Patent Application Laid-Open No. 61-87756
[0012] [Patent document 6] EP59036A1. Summary of the invention
[0013] [Problems to be solved by the invention]
[0014] The first object of the present invention is to provide a novel anthraquinone compound.
[0015] Another object of the present invention is to provide a dichroic dye as the novel anthraquinone compound, a liquid crystal composition containing the dichroic dye, and a light-adjusting element having excellent contrast and light resistance and containing the composition.
[0016] [Technical means to solve the problem]
[0017] The present inventors have successfully obtained novel anthraquinone compounds of specific structures.
[0018] The present inventors have also found that a light control element having excellent contrast and light resistance can be obtained by producing a light control element using a liquid crystal composition containing a dichroic dye as such a novel anthraquinone compound.
[0019] That is, the various aspects included in the present invention are as described below. [1].
[0021] An anthraquinone compound is an anthraquinone compound represented by the following formula (A):
[0022]
[0023] In the formula, R1 represents a branched chain alkyl group having 3 to 16 carbon atoms, and R2 represents a hydrogen atom, a straight chain or branched chain alkyl group having 1 to 8 carbon atoms, or a straight chain or branched chain alkoxy group having 1 to 8 carbon atoms. [2].
[0025] The anthraquinone compound as described in the above item [1], wherein R1 is a branched chain alkyl having 6 to 16 carbon atoms. [3].
[0027] The anthraquinone compound as described in the above item [2], wherein R1 is a branched chain alkyl group represented by the following formula (B),
[0028]
[0029] In the formula, R3 represents a straight-chain alkyl group having 1 to 6 carbon atoms, and R4 represents a straight-chain alkyl group having 1 to 9 carbon atoms; however, the total number of carbon atoms in the straight-chain alkyl group represented by R3 and the total number of carbon atoms in the straight-chain alkyl group represented by R4 is 5 to 15. [4].
[0031] The anthraquinone compound as described in the above item [3], wherein R3 is a methyl group and R4 is a straight-chain alkyl group having 4 to 7 carbon atoms, or R3 is an ethyl group or a propyl group and R4 is a straight-chain alkyl group having 3 to 7 carbon atoms. [5].
[0033] The anthraquinone compound as described in any one of the above items [1] to [4], wherein R2 is a linear alkoxy group having 1 to 8 carbon atoms. [6].
[0035] The anthraquinone compound as described in the above item [5], wherein R2 is a straight-chain alkoxy group having 1 to 4 carbon atoms. [7].
[0037] The anthraquinone compound as described in any one of the above items [1] to [4], wherein R2 is a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms. [8].
[0039] A liquid crystal composition comprising the anthraquinone compound according to any one of the above items [1] to [7] and a liquid crystal material. [9].
[0041] The liquid crystal composition as described in the above item [8] further contains a dichroic dye other than the anthraquinone compound represented by formula (A).
[10] .
[0043] The liquid crystal composition as described in the above item [8] or [9] further contains a photocurable compound and a photopolymerization initiator.
[11] .
[0045] A photocurable material is a photocurable material of the liquid crystal composition described in the above item
[10] .
[12] .
[0047] A dimming element is formed by sandwiching the liquid crystal composition described in the above item [8] or [9] or the photocurable material described in the above item
[11] between a pair of substrates arranged opposite to each other, wherein at least one of the pair of substrates is a transparent substrate having a transparent electrode.
[13] .
[0049] The dimming element as described in the above item
[12] , wherein both of the pair of substrates are transparent substrates having transparent electrodes.
[0050] [Effects of the Invention]
[0051] The anthraquinone compound of the present invention is useful as a dichroic dye for a liquid crystal light-adjusting element. By using a liquid crystal composition containing such a dichroic dye, a light-adjusting element having excellent contrast and light resistance can be obtained. DETAILED DESCRIPTION
[0052] Hereinafter, the present invention will be described in detail.
[0053] The compound (anthraquinone compound) of the present invention is a compound represented by the following formula (A).
[0054]
[0055] In formula (A), R1 represents a branched chain alkyl group having 3 to 16 carbon atoms.
[0056] Specific examples of the branched chain alkyl group having 3 to 16 carbon atoms represented by R1 in formula (A) include isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, isohexyl, tert-pentyl, 1-methylpentyl, 2-methylpentyl, 1-methylhexyl, 2-methylhexyl, 1-methylheptyl, 2-methylheptyl, 1-methyloctyl, 2-methyloctyl, 1-methylnonyl, 2-methylnonyl, 3-methylbutyl, 3-methylpentyl, 3-methylhexyl, 3-methylheptyl, 3-methyloctyl, 1-ethylpropyl, 2-ethylpropyl, 1- R1 is preferably a branched chain alkyl group having 6 to 16 carbon atoms.
[0057] In particular, R1 in the formula (A) is preferably a branched chain alkyl group represented by the following formula (B).
[0058]
[0059] In formula (B), R3 represents a linear alkyl group having 1 to 6 carbon atoms.
[0060] Specific examples of the linear alkyl group having 1 to 6 carbon atoms represented by R3 in formula (B) include methyl, ethyl, n-propyl, n-butyl, n-pentyl and n-hexyl. R3 is preferably methyl, ethyl or n-propyl, and particularly preferably ethyl or n-propyl.
[0061] In formula (B), R4 represents a linear alkyl group having 1 to 9 carbon atoms.
[0062] Specific examples of the straight-chain alkyl group having 1 to 9 carbon atoms represented by R4 include the same specific examples of the straight-chain alkyl group having 1 to 6 carbon atoms represented by R3, as well as n-heptyl, n-octyl and n-nonyl. R4 is more preferably n-propyl, n-butyl, n-pentyl, n-hexyl or n-heptyl.
[0063] However, the total number of carbon atoms in the linear alkyl group represented by R3 and the number of carbon atoms in the linear alkyl group represented by R4 is 5 to 15. That is, the number of carbon atoms in the branched chain alkyl group represented by formula (B) is 6 to 16.
[0064] In formula (B), R3 and R4 are preferably R3 is methyl and R4 is a straight-chain alkyl group having 4 to 7 carbon atoms, or R3 is ethyl or propyl and R4 is a straight-chain alkyl group having 3 to 7 carbon atoms. It is particularly preferred that R3 is ethyl or propyl and R4 is a straight-chain alkyl group having 3 to 7 carbon atoms.
[0065] In formula (A), R2 represents a hydrogen atom, a linear or branched alkyl group having 1 to 8 carbon atoms, or a linear or branched alkoxy group having 1 to 8 carbon atoms.
[0066] Specific examples of the linear or branched chain alkyl group having 1 to 8 carbon atoms represented by R2 of formula (A) include the same linear or branched chain alkyl groups having 3 to 8 carbon atoms as those described in the specific examples of the branched chain alkyl group having 3 to 16 carbon atoms represented by R1 of formula (A) and the same linear or branched chain alkyl groups having 1 to 8 carbon atoms as those described in the specific examples of the linear or branched chain alkyl group having 1 to 9 carbon atoms represented by R4 of formula (B). More preferably, the linear or branched chain alkyl group has 1 to 4 carbon atoms.
[0067] Specific examples of the straight chain or branched chain alkoxy group having 1 to 8 carbon atoms represented by R2 in formula (A) include methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, sec-butoxy, tert-butoxy, n-pentoxy, isopentoxy, neopentoxy, tert-pentoxy, hexyloxy, heptoxy, and octoxy, etc. More preferably, it is a straight chain alkoxy group having 1 to 8 carbon atoms, and particularly preferably a straight chain alkoxy group having 1 to 4 carbon atoms.
[0068] R2 in formula (A) is preferably a hydrogen atom, a straight chain or branched chain alkyl group having 1 to 8 carbon atoms, or a straight chain alkoxy group having 1 to 8 carbon atoms. R2 is particularly preferably a hydrogen atom, a straight chain or branched chain alkyl group having 1 to 4 carbon atoms, or a straight chain alkoxy group having 1 to 4 carbon atoms.
[0069] Preferred specific examples of the compound represented by the above formula (A) include the following.
[0070]
[0071]
[0072]
[0073]
[0074]
[0075]
[0076] The compound represented by the above formula (A) can be synthesized by a conventionally known method such as described in WO87 / 02688.
[0077] The liquid crystal composition of the present invention (hereinafter sometimes referred to as "the composition of the present invention") contains the anthraquinone compound represented by the above formula (A) and a liquid crystal material.
[0078] The order parameter (S value) of the anthraquinone compound represented by the above formula (A) contained in the composition of the present invention is more preferably 0.76 or more, and particularly preferably 0.77 or more.
[0079] In addition, the order parameter (S value) in the present invention is calculated from the following formula recorded in the "Liquid Crystal Device Handbook" (edited by the 142nd Committee of the Japan Society for the Promotion of Science, Nikkan Kogyo Shimbun, 1989) based on the spectroscopic measurement of the dichroic ratio of the anthraquinone compound (dichroic pigment) represented by formula (A).
[0080] S=(A / / -A ⊥ ) / (2A ⊥ +A / / )
[0081] In the formula, “A / / ” and “A ⊥ " represent the absorbance of the pigment with respect to light polarized parallel and perpendicular to the orientation direction of the liquid crystal, respectively. The calculated S value is theoretically a value in the range of 0 to 1, and the closer the value is to 1, the higher the contrast as a host-guest type dimming element.
[0082] The content of the anthraquinone compound represented by the above formula (A) in the liquid crystal composition is not particularly limited, but is preferably 0.5 to 5 parts by mass relative to 100 parts by mass of the liquid crystal material. When a dichroic pigment (described later) other than the compound represented by the formula (A) is used in combination, the total content of the anthraquinone compound represented by the formula (A) and the dichroic pigment other than the compound represented by the formula (A) is preferably 0.5 to 5 parts by mass relative to the above range, that is, relative to 100 parts by mass of the liquid crystal material.
[0083] The liquid crystal material contained in the composition of the present invention is not particularly limited as long as it is a material (compound with liquid crystal) with liquid crystal such as nematic liquid crystal, cholesteric liquid crystal, smectic liquid crystal, etc., wherein nematic liquid crystal is more preferably used. The compound with liquid crystal can be listed as the liquid crystal compound described in Items 154 to 192 and 715 to 722 of the aforementioned "Liquid Crystal Device Handbook" (the 142nd Committee of the Japan Society for the Promotion of Science, Nikkan Kogyo Shimbun, 1989).
[0084] The liquid crystal composition of the present invention may also contain: dichroic pigments other than the anthraquinone compound represented by the above formula (A) or optically active substances such as cholesterol nonanoate that may or may not exhibit a liquid crystal phase, various additives such as ultraviolet absorbers and antioxidants, photocurable compounds and photopolymerization initiators, etc.
[0085] The photocurable compound that may be contained in the composition of the present invention is not particularly limited as long as it is a compound having a functional group that can be polymerized by the action of a photopolymerization initiator described below when irradiated with light. The photocurable compound is preferably a combination of a monofunctional monomer having one polymerizable functional group and a difunctional monomer having two or more polymerizable functional groups.
[0086] The monofunctional monomer of the photocurable compound used in the composition of the present invention has the following functions: it has compatibility with liquid crystal in the composition before light irradiation, and when polymerized by light irradiation, it separates from the liquid crystal to form a hardened phase, and alleviates the interface interaction with the liquid crystal phase. Therefore, when the polarity of the monofunctional monomer is too high, the interface interaction with the liquid crystal phase becomes too strong and hinders the movement of the liquid crystal, so a high driving voltage becomes necessary. Therefore, the polarity of the monofunctional monomer is preferably lower.
[0087] The bifunctional monomer as the photocurable compound used in the composition of the present invention performs the function of phase separation with the liquid crystal to form a hardened phase when polymerized by light irradiation, and stabilizing the separation state with the liquid crystal phase. Therefore, when the polarity of the bifunctional monomer is too high, the interface interaction with the liquid crystal phase becomes too strong and hinders the movement of the liquid crystal, so a high driving voltage becomes necessary. Therefore, the polarity of the bifunctional monomer is preferably lower.
[0088] Examples of the photocurable compound include compounds having a (meth)acrylate group, compounds having a vinyl group, and compounds having an allyl group. Compounds having a (meth)acrylate group are more preferred. That is, it is particularly preferred to use a mono(meth)acrylate compound having one (meth)acrylate group in one molecule and a di(meth)acrylate compound having two (meth)acrylate groups in one molecule.
[0089] In addition, in this specification, the description of "(meth)acrylate" means "methacrylate and / or acrylate".
[0090] The mono(meth)acrylate compound is preferably a mono(meth)acrylate having a linear, cyclic or branched chain alkyl group having 5 to 13 carbon atoms. Specific examples thereof include linear mono(meth)acrylate alkyl esters such as pentyl(meth)acrylate, hexyl(meth)acrylate, heptyl(meth)acrylate, octyl(meth)acrylate, nonyl(meth)acrylate, decyl(meth)acrylate, undecyl(meth)acrylate, dodecyl(meth)acrylate and tridecyl(meth)acrylate; cyclic mono(meth)acrylate alkyl esters such as isoborneol(meth)acrylate; and branched chain mono(meth)acrylate alkyl esters such as 2-methylhexyl(meth)acrylate, 2-ethylhexyl(meth)acrylate, 2-propylhexyl(meth)acrylate, 2-methylheptyl(meth)acrylate, 2-ethylheptyl(meth)acrylate and 2-propylheptyl(meth)acrylate.
[0091] Examples of the di(meth)acrylate compound include 1,4-butanediol di(meth)acrylate, 1,5-pentanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,7-heptanediol di(meth)acrylate, 1,8-octanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, 1,11-undecanediol di(meth)acrylate, 1,12-dodecanediol di(meth)acrylate, and 1,13-tridecanediol di(meth)acrylate. In addition, triethylene glycol di(meth)acrylate and other trialkylene glycol di(meth)acrylates are preferably used.
[0092] When a monofunctional monomer and a difunctional monomer are used in combination, the mass ratio of the monofunctional monomer: the difunctional monomer is preferably 10:90 to 96:4, and particularly preferably 50:50 to 95:5. By setting the amount of the monofunctional monomer to the above ratio range, since the compatibility with the liquid crystal does not become too high, the separation of the polymer (polymer phase) formed by light irradiation and the liquid crystal phase is appropriately caused, and in addition to preventing the gelation of only the monomer, it is easy to form a separated phase of the polymer phase and the liquid crystal phase.
[0093] The compatibility of the photocurable compound contained in the liquid crystal composition of the present invention with the liquid crystal material can be evaluated by visually observing the phase separation caused by the decrease in temperature through a polarizing microscope after the photocurable compound and the liquid crystal material are first miscible, or by measuring the obtained phase separation temperature by DSC or the like. The phase separation temperature of the photocurable compound and the liquid crystal material is preferably in the range of 0 to 50°C, and more preferably in the range of 10 to 40°C. By setting the phase separation temperature to the above range, the compatibility of the photocurable compound and the liquid crystal material in the liquid crystal composition becomes good, and phase separation does not occur after the polymerization of the photocurable compound by light irradiation. As a result, the formed liquid crystal phase does not become too small, which can reduce the driving voltage, and it is easy to maintain the miscible state of the composition until light irradiation.
[0094] The photopolymerization initiator that may be contained in the composition of the present invention is not particularly limited as long as it is a compound that can polymerize the photocurable compound by irradiation with light. It is more preferably a photopolymerization initiator that does not remain in the cured product after irradiation with light and cause the deterioration of the dichroic dye such as the anthraquinone compound represented by formula (A).
[0095] As the photopolymerization initiator, it is more preferable to use an alkylphenone-based photopolymerization initiator such as Darocure 1173, Irgacure 651, or Irgacure 184, or a phosphine oxide-based photopolymerization initiator such as Irgacure TPO.
[0096] When a photocurable compound and a photopolymerization initiator are contained, the blending ratio of the total of the compound represented by formula (A) and the liquid crystal material in the composition of the present invention to the photocurable compound is preferably 90:10 to 50:50, more preferably 80:20 to 50:50, and more preferably 65:35 to 50:50 in terms of mass ratio. By setting the blending ratio of the photocurable compound to the above range, separation of the liquid crystal material and the photocurable compound and reduction in light shielding properties of the cured product can be prevented before curing by light irradiation.
[0097] In addition, when a dichroic dye (described later) other than the compound represented by formula (A) is used in combination, the total ratio of all dichroic dyes and liquid crystal materials containing the compound represented by formula (A) to the photocurable compound in the composition of the present invention is preferably in the above range (90:10 to 50:50 in terms of mass ratio). The particularly preferred range and the more preferred range are also the same as above.
[0098] When the photocurable compound and the photopolymerization initiator are contained, the content of the photopolymerization initiator in the composition of the present invention is preferably 0.1 to 5 parts by mass based on 100 parts by mass of the photocurable compound.
[0099] By using a dichroic dye other than the compound represented by the above formula (A) in the composition of the present invention in combination, the contrast of the light-adjusting element during light shielding can be improved.
[0100] The dichroic dyes that can be used in combination are not particularly limited, and can be selected from, for example, azo dyes, anthraquinone dyes, perylene dyes, quinophthalone dyes, merocyanine dyes, azomethine dyes, phthaloperylene dyes, indigo dyes, azulene dyes, dioxazine dyes, polythiophene dyes, etc. Specifically, the dichroic dyes described in "Dichroic dyes for Liquid Crystal Display" (by AVIvashchenko, CRC, 1994) can be cited.
[0101] Among these, it is more preferred to use an azo dye, an anthraquinone dye, a perylene dye or a quinoline yellow dye in combination, and it is particularly preferred to use an azo dye and an anthraquinone dye in combination.
[0102] When a dichroic pigment other than the compound represented by formula (A) is used in combination, the content of the compound represented by formula (A) in the total dichroic pigment is not particularly limited as long as it is within the range that does not impair the effect of the present invention. The amount is preferably 1 to 95% by mass, particularly preferably 10 to 90% by mass, and more preferably 30 to 80% by mass.
[0103] In the composition of the present invention, the following may be used in combination: benzotriazole-based, benzophene-based, and hindered amine-based light stabilizers, phosphite-based and hindered phenol-based antioxidants, thermal polymerization inhibitors, thiol compounds, photosensitizers, photosensitizers, chain transfer inhibitors, polymerization inhibitors, bonding agents, defoamers, crosslinking agents, surfactants, heat-curing accelerators, thermoplastic resins, thermosetting resins, diacrylate urethane and other tackifiers, etc.
[0104] In order to control the cell gap as a light-adjusting element, a spherical or cylindrical spacer such as silicon oxide, glass, plastic, or ceramic may be added. In this case, the cell gap may be set within a range of 2 to 100 μm.
[0105] The composition of the present invention is obtained by mixing and stirring the anthraquinone compound represented by formula (A) as an essential component and a liquid crystal material, and any components such as a photocurable compound and a photopolymerization initiator added as needed. The mixing and stirring can be simply carried out by putting all the components into a container and stirring them manually, but it is more effective to use a machine such as a magnetic stirrer for stirring. In addition, in order to efficiently prepare a uniform composition, it is more preferred to first prepare a uniform mixture of a photocurable compound, a photopolymerization initiator and a liquid crystal material, and then add the compound represented by formula (A) and any other components and stir and mix them. During the stirring and mixing, heating can also be applied as needed. The stirring and mixing under a light source that emits the absorption wavelength of the photopolymerization initiator is preferably carried out in a very short time. After mixing the components, filtering can be performed using a sieve, a membrane filter, etc.
[0106] By irradiating light to the composition of the present invention containing a photocurable compound and a photopolymerization initiator, a cured product of a liquid crystal composition in which the photocurable compound component is cured (polymerized) is obtained. In addition, the "cured product" in the present invention means a state in which the functional groups of the photocurable compound are polymerized or copolymerized by irradiation with light, and does not mean a cured product in which the anthraquinone compound represented by formula (A) or the liquid crystal material necessarily participates in the curing reaction.
[0107] The light source for irradiating light is not particularly limited as long as it can irradiate light of a wavelength absorbed by the photopolymerization initiator. Preferred light sources include high-pressure mercury lamps, metal halide lamps, xenon lamps, and halogen lamps that can irradiate ultraviolet rays.
[0108] The temperature during light irradiation is preferably set to a temperature at which the composition can be maintained in a uniformly miscible state, that is, a temperature higher than the phase separation temperature, and is particularly preferably set to a temperature range of 1 to 5°C higher than the phase separation temperature. By setting the temperature during light irradiation higher than the phase separation temperature, it is possible to prevent the photocurable compound and the liquid crystal material from being separated before irradiation, thereby obtaining a more uniform cured product. On the other hand, by not setting the temperature during light irradiation significantly higher than the phase separation temperature, when the polymer of the photocurable compound obtained by light curing separates from the liquid crystal material, it is possible to prevent the size of the crystal domain formed by the liquid crystal material from becoming too small.
[0109] The dimming element of the present invention is a transparent substrate in which a layer of the liquid crystal composition of the present invention or a photocured material of the liquid crystal composition is sandwiched between a pair of substrates arranged opposite to each other, and at least one of the pair of substrates has a transparent electrode. Here, the substrate can be, for example, an inorganic transparent material such as glass or quartz, a metal, a metal oxide, a semiconductor, a ceramic, a plastic plate, a plastic film, etc., which is colorless, transparent, colored, transparent, or opaque. The electrode is formed on the substrate by a known coating method, a printing method, or a vapor deposition method such as sputtering, etc., such as a thin film of a metal oxide, a metal, a semiconductor, an organic conductive material, etc., on the entire or a part of the substrate. In particular, in order to obtain a dimming element of a large area, it is more preferable from the perspective of productivity and processability to use an electrode substrate in which an ITO (indium oxide, tin oxide) electrode is formed on a transparent polymer film such as PET by a vapor deposition method such as sputtering, or a printing method. A particularly preferred aspect is a transparent substrate in which both of the pair of substrates have transparent electrodes. Wiring for connecting the electrode or the electrode to the outside may also be provided on the substrate. For example, a segmented driving electrode substrate, a matrix driving electrode substrate, an active matrix driving electrode substrate, etc. can be used. In addition, the electrode surface provided on the substrate can also be fully or partially covered by a protective film or an alignment film composed of organic compounds such as polyimide, polyamide, polysilicon, and cyanide compounds; inorganic compounds such as SiO2, TiO2, and ZrO2; or a mixture of these.
[0110] By using a plastic film as a substrate, a flexible and lightweight dimming element is obtained. Therefore, the dimming element can be clamped between a pair of flat or curved glass or hard plastics, etc., through a bonding layer such as polyvinyl butyral or vinyl acetate, double-sided tape, adhesive, etc., and used. Or the dimming element can be attached to the surface of a flat or curved glass or hard plastic, etc. through a double-sided tape or adhesive, etc. and used. In addition, it can also be sandwiched between soft plastics and attached to one side or both sides. In addition, a hard coating, an ultraviolet blocking layer or an infrared blocking layer, a semi-reflecting mirror, etc. protective layers can also be provided on the substrate surface of the dimming element on the opposite side of the electrode surface, and a color filter can also be stacked or a polarizing filter can be attached. In addition, it can also be stacked as an electroluminescent display element, a light-emitting diode display element, an electrochromic display element, and other liquid crystal display elements.
[0111] The driving device used to apply voltage to the dimming element of the present invention is a device that can apply a DC voltage of 2 to 100V or an AC voltage of 10 to 1000Hz. When no voltage is applied, it is only necessary to disconnect or short-circuit the electrodes. In addition, this driving device may also have a voltage application circuit for segmented driving, a voltage application circuit for matrix driving, a voltage application circuit for active matrix, etc.
[0112] The dimming element of the present invention may be any one of a black dimming element and a color dimming element depending on the application. The average transmittance of the dimming element of the present invention when light is transmitted in a specific wavelength region is preferably 35% or more, and more preferably 40% or more. In addition, the average transmittance when blocking light is preferably 25% or less, and more preferably 15% or less.
[0113] The black dimming element has a neutral color, has little color leakage and excellent contrast in the visible light region when no voltage is applied, and has excellent light resistance when exposed outdoors for a long period of time, so it is most suitable for automotive use or building material use.
[0114] [Example]
[0115] The present invention is described in more detail below by way of examples, but these are merely illustrative and do not limit the present invention. In addition, "parts" and "%" herein are by mass unless otherwise specified. The maximum absorption wavelength in the examples is a value measured by a spectrophotometer "UV-3150" manufactured by Shimadzu Corporation.
[0116] Example 1 (Synthesis of the compound represented by formula (5) of the specific example)
[0117] (Step 1) Synthesis of the intermediate compound represented by formula (47)
[0118] 10.0 parts of 1,5-dichloroanthraquinone, 7.3 parts of potassium carbonate and 6.0 parts of 4-hydroxybenzenethiol were added to 120 parts of DMF and stirred at 60°C for 4 hours. After the reaction solution was cooled to 25°C, 240 parts of methanol was added and stirred for 1 hour. The reaction product was filtered and dried in a hot air dryer at 80°C for 24 hours to obtain 6.3 parts of an intermediate compound represented by the following formula (47).
[0119]
[0120] (Step 2) Synthesis of the intermediate compound represented by formula (48)
[0121] 6.3 parts of the intermediate compound represented by the formula (47) obtained in step 1, 3.6 parts of potassium carbonate and 4.3 parts of 4-tert-butylbenzenethiol were added to 70 parts of DMF and stirred at 60°C for 2 hours. After the reaction solution was cooled to 25°C, 140 parts of methanol was added and stirred for 1 hour. The reaction product was filtered and washed with toluene, and then dried in a hot air dryer at 80°C for 24 hours to obtain 5.1 parts of the intermediate compound represented by the following formula (48).
[0122]
[0123] (Step 3) Synthesis of the compound of the present invention represented by formula (5)
[0124] 5.1 parts of the intermediate compound represented by formula (48) obtained in step 2, 1.6 parts of 2-methylhexanoyl chloride and 1.8 parts of triethylamine were added to 70 parts of toluene, and after stirring at 25°C for 1 hour, 40 parts of water were added to separate the organic phase. After the aqueous layer was extracted with 60 parts of ethyl acetate, the separated organic layer and the ethyl acetate extract were mixed and washed with 70 parts of saturated brine. After the washed organic layer was dried over anhydrous magnesium sulfate, the crude product obtained by vacuum distillation of the solvent was dissolved in toluene, and column purification was performed using toluene as an extended solvent. The solvent was vacuum distilled from the refined solution and dried in a hot air dryer at 80°C for 24 hours, thereby obtaining 3.5 parts of the compound represented by the above formula (5) as an orange solid. The maximum absorption wavelength of the toluene solution of this compound is 448nm.
[0125] Example 2 (Synthesis of the Compound Represented by Formula (7) of Specific Example)
[0126] The same operation as in Example 1 was carried out except that 1.6 parts of 2-methylhexanoyl chloride in step 3 was replaced with 2.2 parts of 2-ethylhexanoyl chloride to obtain 3.8 parts of the compound represented by the above formula (7) as an orange solid. The maximum absorption wavelength of the toluene solution of this compound was 448 nm.
[0127] Example 3 (Synthesis of the Compound Represented by Formula (12) of Specific Example)
[0128] The same operation as in Example 1 was carried out except that 4.3 parts of 4-tert-butylbenzenethiol in step 2 was replaced by 3.2 parts of 4-methylbenzenethiol, and 1.6 parts of 2-methylhexanoyl chloride in step 3 was replaced by 2.2 parts of 2-ethylhexanoyl chloride, to obtain 2.8 parts of the compound represented by the above formula (12) as an orange solid. The maximum absorption wavelength of the toluene solution of this compound is 449 nm.
[0129] Example 4 (Synthesis of the Compound Represented by Formula (21) of Specific Example)
[0130] The same operation as in Example 1 was carried out except that 4.3 parts of 4-tert-butylbenzenethiol in step 2 was replaced by 5.8 parts of n-octanethiol and 1.6 parts of 2-methylhexanoyl chloride in step 3 was replaced by 1.6 parts of 5-methylhexanoyl chloride, to obtain 3.1 parts of the compound represented by the above formula (21). The maximum absorption wavelength of the toluene solution of this compound is 448 nm.
[0131] Example 5 (Synthesis of the Compound Represented by Formula (28) of Specific Example)
[0132] The same operation as in Example 1 was carried out except that 4.3 parts of 4-tert-butylbenzenethiol in step 2 was replaced by 4.2 parts of n-butoxybenzenethiol and 1.6 parts of 2-methylhexanoyl chloride in step 3 was replaced by 1.6 parts of 2-ethylheptanoyl chloride, to obtain 2.7 parts of the compound represented by the above formula (28). The maximum absorption wavelength of the toluene solution of this compound is 453 nm.
[0133] Synthesis Example 1 (Synthesis of Comparative Compound)
[0134] The compound represented by No. 8 in Table 1 of JP-A-61-87756 (a compound represented by the following formula (X)) was obtained by a generally known synthesis method.
[0135]
[0136] Synthesis Example 2 (Synthesis of Comparative Compound)
[0137] The compound represented by Example 11 of EP59036A1 (a compound represented by the following formula (Y)) was obtained by a generally known synthesis method.
[0138]
[0139] Example 6 (Preparation of the composition of the present invention)
[0140] 0.0078 parts of the compound represented by formula (5) obtained in Example 1, 0.306 parts of 1-cyano-4'-n-pentylbiphenyl, 0.15 parts of 1-cyano-4'-n-heptylbiphenyl, 0.096 parts of 1-cyano-4'-n-octyloxybiphenyl and 0.048 parts of 1-cyano-4"-n-pentylterphenyl were mixed at room temperature to prepare the liquid crystal composition of the present invention.
[0141] Examples 7 to 10 and Comparative Examples 1 and 2 (Preparation of Liquid Crystal Compositions of the Invention and Comparative Examples)
[0142] Except for changing the compound represented by formula (5) obtained in Example 1 to the compound represented by formula (7) obtained in Example 2, the compound represented by formula (12) obtained in Example 3, the compound represented by formula (21) obtained in Example 4, the compound represented by formula (28) obtained in Example 5, the compound represented by formula (X) obtained in Synthesis Example 1 and the compound represented by formula (Y) obtained in Synthesis Example 2, the liquid crystal composition of the present invention and the comparative liquid crystal composition were respectively prepared according to Example 6.
[0143] Examples 11 to 15 and Comparative Examples 3 and 4 (Fabrication of the Light-Adjusting Components of the Invention and Comparative Examples)
[0144] The liquid crystal compositions obtained in Examples 6 to 10 and Comparative Examples 1 and 2 were sealed in a device with a gap of 15 μm between the substrates. The device was composed of two glass substrates, upper and lower, with transparent electrodes and subjected to horizontal alignment treatment by brushing polyamide resin on the surface in contact with the liquid crystal. In the aforementioned device, the liquid crystal was in a horizontal alignment state when no voltage was applied, and the pigment molecules also followed the liquid crystal and were in the same alignment state.
[0145] (Calculation of Order Parameters of Light Adjusting Element)
[0146] Linear polarization parallel to the alignment direction and linear polarization perpendicular to the alignment direction were incident on the dimming elements obtained in Examples 11 to 15 and Comparative Examples 3 and 4. From the respective spectra at this time, the absorbance (A) of the colored unit with respect to the linear polarization parallel to the alignment direction was measured. / / ) and the absorbance relative to polarized light perpendicular to the alignment direction (A ⊥ ), and the order parameter (S value) at the maximum absorption wavelength (λmax) was obtained from the following formula. The results are shown in Table 1.
[0147] S=(A / / -A ⊥ ) / (2A ⊥ +A / / )
[0148] [Table 1]
[0149] Table 1 Calculation results of order parameter (S value)
[0150]
[0151]
[0152] As shown in Table 1, the dimming elements of Examples 11 to 15 have higher order parameters than the dimming elements of Comparative Examples 3 and 4, and thus are superior as dimming elements.
[0153] (Light resistance test of dimming components)
[0154] A UV cut filter with a wavelength of 400 nm or less was attached to the dimming elements obtained in Examples 11 to 15 and Comparative Example 3, and the light was filtered at 63°C with an illumination of 650 W / m 2After 200 hours of light irradiation with a metal halide lamp, the S value at this time was measured. In the following Table 2, the S value of the dimming element of each example before light irradiation (the value shown in the above Table 1) and the S value after 200 hours of light irradiation are shown together. As shown in Table 2, the S value of the dimming element of Examples 11 to 15 changes little over time, but the S value of the dimming element of Comparative Example 3 decreases significantly after 200 hours. From this result, it is confirmed that the dimming elements of Examples 11 to 15 have excellent light resistance.
[0155] [Table 2]
[0156] Table 2 Lightfastness test results
[0157]
[0158]
[0159] Example 16 (Preparation of the Liquid Crystal Composition of the Present Invention)
[0160] 0.026 parts of the compound represented by the above formula (5) obtained in Example 1, 0.380 parts of isobornyl acrylate (manufactured by Osaka Organic Chemical Industry Co., Ltd., monoacrylate), 0.020 parts of triethylene glycol dimethacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd.), 0.306 parts of 1-cyano-4'-n-pentylbiphenyl, 0.15 parts of 1-cyano-4'-n-heptylbiphenyl, 0.096 parts of 1-cyano-4'-n-octyloxybiphenyl, 0.048 parts of 1-cyano-4"-n-pentylterphenyl, 0.004 parts of Irgacure TPO (manufactured by BASF), 0.004 parts of Irgacure 184 (manufactured by BASF), and 0.010 parts of a spacer agent having a diameter of 20 μm (Micropearl (registered trademark) SP220 manufactured by Sekisui Chemical Co., Ltd.) were mixed at room temperature to prepare a liquid crystal composition of the present invention.
[0161] Examples 17 to 20 and Comparative Example 5 (Preparation of Liquid Crystal Compositions of the Invention and Comparative Examples)
[0162] The liquid crystal composition of the present invention and the comparative liquid crystal composition were obtained according to Example 16, except that 0.026 parts of the compound represented by formula (5) obtained in Example 1 were changed to 0.026 parts of the compound represented by formula (7) obtained in Example 2, 0.026 parts of the compound represented by formula (12) obtained in Example 3, 0.026 parts of the compound represented by formula (21) obtained in Example 4, 0.026 parts of the compound represented by formula (28) obtained in Example 5, and 0.007 parts of the compound represented by formula (X) obtained in Synthesis Example 1. 0.007 parts of the compound represented by formula (X) obtained in Synthesis Example 1 was the maximum solubility in the liquid crystal mixture.
[0163] Examples 21 to 25 and Comparative Example 6 (Fabrication of the Dimming Element of the Invention and Comparative Example)
[0164] On the ITO film of the 5 cm square PET film provided with the ITO film, the liquid crystal compositions obtained in Examples 16 to 20 and Comparative Example 5 were coated using a coater to form a liquid crystal composition layer. Next, this film and the same 5 cm square PET film provided with the ITO film as described above were overlapped in such a way that the liquid crystal composition layer on the ITO film and the ITO film were opposed to each other. Then, the sample of the laminate of the two films and the liquid crystal composition layer thus obtained was maintained at 23° C. on a hot plate and set at a light intensity of 9 mW / cm at 365 nm of an LED lamp. 2 , and light irradiation was performed for 1 minute to photocure the photocurable compound, thereby obtaining a dimming element of the present invention and a comparative dimming element, respectively.
[0165] (Calculation of contrast of dimming element)
[0166] The maximum absorption wavelength was measured for the dimming elements obtained in Examples 21 to 25 and Comparative Example 6, and the comparison (transmittance when voltage was applied / transmittance when voltage was not applied) was calculated from the measurement results of the transmittance at the maximum absorption wavelength when 100V AC voltage (50Hz sine wave) was applied and when it was not applied. The results are shown in Table 3.
[0167] [Table 3]
[0168] Table 3 Comparison results
[0169]
[0170] As shown in Table 3, the dimming elements of Examples 21 to 25 have a contrast ratio of about 2 times or more than 2 times that of the dimming element of Comparative Example 6. In addition, the dimming elements of Examples 21 to 25 have a transmittance when shielding light that is 20% or more lower than that of the dimming element of Comparative Example 6, and have excellent light shielding performance. Therefore, it can be clearly understood that the dimming elements of Examples 21 to 25 exhibit more excellent performance than the dimming element of Comparative Example 6.
[0171] (Light resistance test of dimming components)
[0172] A UV cut filter with a wavelength of 400 nm or less was attached to the dimming elements obtained in Examples 21 to 25 and Comparative Example 6, and the light was filtered at 63°C with an illumination of 650 W / m 2After 24 hours of light irradiation with a metal halide lamp, the absorbance at the maximum absorption wavelength was measured and the absorbance retention rate ((δA)%) was calculated. The absorbance retention rate ((δA)%) is defined by the following formula, where the absorbance value before light irradiation (i.e., 0 hours after light irradiation) is A(0) and the absorbance value after 24 hours of light irradiation is A(24). The larger the δA value, the better the light resistance.
[0173] (δA)%=(A(24) / A(0))×100
[0174] The maximum absorption wavelength and the absorbance retention rate of the dimming element of each example are shown in Table 4. As shown in Table 4, the absorbance retention rate of the dimming elements of Examples 21 to 25 is greatly improved compared with the dimming element of Comparative Example 6. Therefore, it can be clearly understood that the dimming elements of Examples 21 to 25 exhibit better light resistance than the dimming element of Comparative Example 6.
[0175] [Table 4]
[0176] Table 4 Lightfastness test results
[0177]
[0178]
[0179] Example 26 (Fabrication of Black Dimming Element)
[0180] The liquid crystal composition of the present invention was prepared in the same manner as in Example 16, except that 0.026 parts of the compound represented by formula (5) obtained in Example 1 was replaced by 0.009 parts of the compound represented by formula (7) obtained in Example 2, and 0.012 parts of LCD121 (anthraquinone compound, manufactured by Nippon Kayaku Co., Ltd.) and 0.009 parts of LCD212 (anthraquinone compound, manufactured by Nippon Kayaku Co., Ltd.) were added. A black dimming element was prepared using the liquid crystal composition in the same manner as in Examples 21 to 25. The obtained black dimming element had an average contrast ratio of 3.5 at 400 to 700 nm, showing a high contrast ratio.
[0181] The black dimming element obtained in Example 26 showed no change in transmittance even after 500 hours in the xenon light resistance test, and also had excellent light resistance when exposed to light for a long time. This result indicates that the black dimming element of Example 26 is a black liquid crystal dimming element with high contrast and light resistance.
[0182] [Industrial Applicability]
[0183] By using the liquid crystal composition of the present invention, a light-adjusting liquid crystal element having high contrast and high light resistance can be obtained, and can be suitably used in outdoor building materials and vehicle applications requiring high durability.
Claims
1. An anthraquinone compound, which is an anthraquinone compound represented by the following formula (A): In the formula, R1 represents a branched alkyl group having 6 to 16 carbon atoms, and R2 represents a hydrogen atom, a straight-chain or branched alkyl group having 1 to 8 carbon atoms, or a straight-chain or branched alkoxy group having 1 to 8 carbon atoms.
2. The anthraquinone compound according to claim 1, wherein R1 is a branched alkyl group represented by the following formula (B), In the formula, R3 represents a straight-chain alkyl group having 1 to 6 carbon atoms, and R4 represents a straight-chain alkyl group having 1 to 9 carbon atoms; however, the total number of carbon atoms in the straight-chain alkyl group represented by R3 and the total number of carbon atoms in the straight-chain alkyl group represented by R4 is 5 to 15.
3. The anthraquinone compound according to claim 2, wherein R3 is a methyl group and R4 is a straight-chain alkyl group having 4 to 7 carbon atoms, or R3 is an ethyl group or a propyl group and R4 is a straight-chain alkyl group having 3 to 7 carbon atoms.
4. The anthraquinone compound according to any one of claims 1 to 3, wherein R2 is a linear alkoxy group having 1 to 8 carbon atoms.
5. The anthraquinone compound according to claim 4, wherein R2 is a linear alkoxy group having 1 to 4 carbon atoms.
6. The anthraquinone compound according to any one of claims 1 to 3, wherein R2 is a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms. 7 . A liquid crystal composition comprising the anthraquinone compound according to claim 1 and a liquid crystal material. 8 . The liquid crystal composition according to claim 7 , further comprising a dichroic dye other than the anthraquinone compound represented by formula (A). 9 . The liquid crystal composition according to claim 7 , further comprising a photocurable compound and a photopolymerization initiator. 10 . A photocured product, which is a photocured product of the liquid crystal composition according to claim 9 .
11. A light-adjusting element, comprising: a liquid crystal composition according to claim 7 or 8 or a light-cured material according to claim 10 sandwiched between a pair of substrates disposed opposite to each other, wherein at least one of the pair of substrates is a transparent substrate having a transparent electrode.
12. The dimming element according to claim 11, wherein: Both of the pair of substrates are transparent substrates having transparent electrodes.
Citation Information
Patent Citations
Pleochroic anthraquinone dyes
EP0059036A1
Reconfigurable microdisplay
EP1350136A1
Method of manufacturing a liquid crystal light modulating material
JP1988501512A
Liquid crystal panel
JP1991047392A
Liquid crystal composition for light control, photo-cured product thereof, and light control element