A polycarboxylate water reducer and preparation method thereof

By adding a composite solubilizer of diethyl maleate and sodium tripolyphosphate in the preparation of polycarboxylate water-reducing agent, the problem of insufficient fluidity of cement material slurry in the existing technology is solved, and its dispersion performance is significantly improved. .

CN117105569BActive Publication Date: 2024-10-11HUNAN SUNNY TRADE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311232488.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-22
Publication Date
2024-10-11
Estimated Expiration
2043-09-22

AI Technical Summary

Technical Problem

Existing polycarboxylate superplasticizers are insufficient in improving the fluidity of cement materials, and the effect of using diethyl maleate or sodium tripolyphosphate alone is limited.

Method used

During the preparation process of the polycarboxylate water-reducing agent, a composite solubilizer composed of diethyl maleate and sodium tripolyphosphate is added, and the pH value of the product is adjusted through specific reaction steps and temperature control to improve its dispersion performance.

Benefits of technology

The fluidity of the cement slurry is significantly improved. The effect of the composite solubilizer is better than that of diethyl maleate or sodium tripolyphosphate used alone, and the dispersion performance of the water reducing agent is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004464393690000041
    Figure BDA0004464393690000041
Patent Text Reader

Abstract

The invention discloses a polycarboxylate water reducer and a preparation method thereof. In order to improve the fluidity of the cement paste, the invention adds a composite solubilizer composed of diethyl maleate / sodium tripolyphosphate during the preparation of the polycarboxylate water reducer. Studies have shown that the addition of the composite solubilizer can significantly improve the fluidity of the cement paste, and the test effect of the composite solubilizer is better than that of diethyl maleate or sodium tripolyphosphate used alone.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of water reducing agents, and in particular to a polycarboxylic acid water reducing agent and a preparation method thereof. Background Art

[0002] Polycarboxylate superplasticizer, also known as polycarboxylate superplasticizer, is a series of superplasticizers made by copolymerizing unsaturated monomers containing carboxylic acid and other monomers, which makes concrete have excellent performance in water reduction, slump retention, plasticization, shrinkage and environmental protection. Polycarboxylate superplasticizers are widely used due to their advantages such as low dosage, high water reduction rate, good slump retention, high compressive strength ratio, green environmental protection, high durability and cost saving. However, improving the relevant performance of polycarboxylate superplasticizers has been a long-term goal in this field. Summary of the invention

[0003] In view of the problems existing in the prior art, the present invention aims to provide a method for preparing a polycarboxylate water-reducing agent.

[0004] A method for preparing a polycarboxylate water-reducing agent comprises the following steps:

[0005] Add 35-40 parts by weight of isopentanol polyoxyethylene ether, 100-120 parts by weight of acrylic acid, 0.5-3 parts by weight of diethyl maleate, 0.5-3 parts by weight of sodium tripolyphosphate and 200-220 parts by weight of deionized water to the reaction kettle in sequence, heat the temperature to 60-72° C., and keep warm for 15-30 minutes;

[0006] 5.5-6.0 parts by weight of K2S2O8 aqueous solution was uniformly added dropwise to the reaction kettle, and the reaction was kept warm for 15-30 minutes, and then 3.0-3.2 parts by weight of mercaptoethanol aqueous solution was uniformly added dropwise to the reaction kettle, and the reaction was kept warm for 30-45 minutes;

[0007] The heating was stopped and the mixture was cooled naturally to room temperature, and the pH value of the product was adjusted to 6.8-7.0 using an alkaline solution.

[0008] Preferably, the alkaline solution is KOH.

[0009] Preferably, the alkaline solution is NaOH.

[0010] Preferably, the pH value is 6.8.

[0011] Preferably, the amount of the isopentanol polyoxyethylene ether is 35 parts by weight.

[0012] Preferably, the amount of acrylic acid used is 100 parts by weight.

[0013] Preferably, the amount of K2S2O8 used is 5.5 parts by weight.

[0014] Furthermore, the present invention also provides a polycarboxylate water-reducing agent, which is prepared by any of the above methods.

[0015] In order to improve the fluidity of cement paste, the present invention adds a composite solubilizer composed of diethyl maleate / sodium tripolyphosphate in the preparation process of polycarboxylate water-reducing agent. Studies have shown that the addition of the composite solubilizer can significantly improve the fluidity of cement paste, and the test effect of the composite solubilizer is better than that of diethyl maleate or sodium tripolyphosphate used alone. DETAILED DESCRIPTION

[0016] The technical effects of the present invention are verified below through specific examples, but the embodiments of the present invention are not limited thereto.

[0017] In the present invention, the weight parts of the aqueous solution represent the weight parts of the effective substance. For example, 5.5 weight parts of K2S2O8 aqueous solution represent 5.5 weight parts of K2S2O8.

[0018] Example 1

[0019] 35 parts by weight of isopentanol polyoxyethylene ether, 100 parts by weight of acrylic acid, 0.5 parts by weight of diethyl maleate, 0.5 parts by weight of sodium tripolyphosphate and 200 parts by weight of deionized water were added to the reaction kettle in sequence, and the temperature was heated to 72° C. and kept warm for 30 minutes;

[0020] 5.5 parts by weight of K2S2O8 aqueous solution were uniformly added dropwise to the reaction kettle, and the reaction was kept warm for 30 minutes. Then 3.2 parts by weight of mercaptoethanol aqueous solution were uniformly added dropwise to the reaction kettle, and the reaction was kept warm for 45 minutes.

[0021] The heating was stopped and the mixture was cooled to room temperature naturally, and the pH value of the product was adjusted to 6.8 using KOH solution.

[0022] Example 2

[0023] 35 parts by weight of isopentanol polyoxyethylene ether, 100 parts by weight of acrylic acid, 1.2 parts by weight of diethyl maleate, 1.2 parts by weight of sodium tripolyphosphate and 200 parts by weight of deionized water were added to the reaction kettle in sequence, and the temperature was heated to 72° C. and kept warm for 30 minutes;

[0024] 5.5 parts by weight of K2S2O8 aqueous solution were uniformly added dropwise to the reaction kettle, and the reaction was kept warm for 30 minutes. Then 3.2 parts by weight of mercaptoethanol aqueous solution were uniformly added dropwise to the reaction kettle, and the reaction was kept warm for 45 minutes.

[0025] The heating was stopped and the mixture was cooled to room temperature naturally, and the pH value of the product was adjusted to 6.8 using KOH solution.

[0026] Example 3

[0027] 35 parts by weight of isopentanol polyoxyethylene ether, 100 parts by weight of acrylic acid, 1.9 parts by weight of diethyl maleate, 1.4 parts by weight of sodium tripolyphosphate and 200 parts by weight of deionized water were added to the reaction kettle in sequence, and the temperature was heated to 72° C. and kept warm for 30 minutes;

[0028] 5.5 parts by weight of K2S2O8 aqueous solution were uniformly added dropwise to the reaction kettle, and the reaction was kept warm for 30 minutes. Then 3.2 parts by weight of mercaptoethanol aqueous solution were uniformly added dropwise to the reaction kettle, and the reaction was kept warm for 45 minutes.

[0029] The heating was stopped and the mixture was cooled to room temperature naturally, and the pH value of the product was adjusted to 6.8 using KOH solution.

[0030] Example 4

[0031] 35 parts by weight of isopentanol polyoxyethylene ether, 100 parts by weight of acrylic acid, 1.4 parts by weight of diethyl maleate, 1.9 parts by weight of sodium tripolyphosphate and 200 parts by weight of deionized water were added to the reaction kettle in sequence, and the temperature was heated to 72° C. and kept warm for 30 minutes;

[0032] 5.5 parts by weight of K2S2O8 aqueous solution were uniformly added dropwise to the reaction kettle, and the reaction was kept warm for 30 minutes. Then 3.2 parts by weight of mercaptoethanol aqueous solution were uniformly added dropwise to the reaction kettle, and the reaction was kept warm for 45 minutes.

[0033] The heating was stopped and the mixture was cooled to room temperature naturally, and the pH value of the product was adjusted to 6.8 using KOH solution.

[0034] Example 5

[0035] 35 parts by weight of isopentanol polyoxyethylene ether, 100 parts by weight of acrylic acid, 3 parts by weight of diethyl maleate, 3 parts by weight of sodium tripolyphosphate and 200 parts by weight of deionized water were added to the reaction kettle in sequence, and the temperature was heated to 72° C. and kept warm for 30 minutes;

[0036] 5.5 parts by weight of K2S2O8 aqueous solution were uniformly added dropwise to the reaction kettle, and the reaction was kept warm for 30 minutes. Then 3.2 parts by weight of mercaptoethanol aqueous solution were uniformly added dropwise to the reaction kettle, and the reaction was kept warm for 45 minutes.

[0037] The heating was stopped and the mixture was cooled to room temperature naturally, and the pH value of the product was adjusted to 6.8 using KOH solution.

[0038] Comparative Example 1

[0039] 35 parts by weight of isopentanol polyoxyethylene ether, 100 parts by weight of acrylic acid, 3.3 parts by weight of diethyl maleate and 200 parts by weight of deionized water were added to the reaction kettle in sequence, and the temperature was heated to 72° C. and kept warm for 30 minutes;

[0040] 5.5 parts by weight of K2S2O8 aqueous solution were uniformly added dropwise to the reaction kettle, and the reaction was kept warm for 30 minutes. Then 3.2 parts by weight of mercaptoethanol aqueous solution were uniformly added dropwise to the reaction kettle, and the reaction was kept warm for 45 minutes.

[0041] The heating was stopped and the mixture was cooled to room temperature naturally, and the pH value of the product was adjusted to 6.8 using KOH solution.

[0042] Comparative Example 2

[0043] 35 parts by weight of isopentanol polyoxyethylene ether, 100 parts by weight of acrylic acid, 3.3 parts by weight of sodium tripolyphosphate and 200 parts by weight of deionized water were added to the reaction kettle in sequence, and the temperature was heated to 72° C. and kept warm for 30 minutes;

[0044] 5.5 parts by weight of K2S2O8 aqueous solution were uniformly added dropwise to the reaction kettle, and the reaction was kept warm for 30 minutes. Then 3.2 parts by weight of mercaptoethanol aqueous solution were uniformly added dropwise to the reaction kettle, and the reaction was kept warm for 45 minutes.

[0045] The heating was stopped and the mixture was cooled to room temperature naturally, and the pH value of the product was adjusted to 6.8 using KOH solution.

[0046] Comparative Example 3

[0047] 35 parts by weight of isopentanol polyoxyethylene ether, 100 parts by weight of acrylic acid and 200 parts by weight of deionized water were added to the reaction kettle in sequence, and the temperature was heated to 72° C. and kept warm for 30 minutes;

[0048] 5.5 parts by weight of K2S2O8 aqueous solution were uniformly added dropwise to the reaction kettle, and the reaction was kept warm for 30 minutes. Then 3.2 parts by weight of mercaptoethanol aqueous solution were uniformly added dropwise to the reaction kettle, and the reaction was kept warm for 45 minutes.

[0049] The heating was stopped and the mixture was cooled to room temperature naturally, and the pH value of the product was adjusted to 6.8 using KOH solution.

[0050] Hereinafter, the inventors evaluated the dispersibility of the polycarboxylate water-reducing agent in Examples 1-5 and Comparative Examples 1-3 by the fluidity of cement paste, and the test method was carried out in accordance with GB / T8077-2012, and the water-reducing agent was added in a solid content of 0.18%. The test results are shown in Table 1.

[0051] Table 1

[0052]

[0053] According to the experimental results in Table 1, it can be seen that the present invention can significantly improve the dispersibility of the water reducing agent after adding the composite solubilizer (diethyl maleate / sodium tripolyphosphate).

[0054] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a polycarboxylate water-reducing agent, It is characterized in that The preparation method of the polycarboxylate water-reducing agent comprises the following steps: 35 parts by weight of isopentanol polyoxyethylene ether, 100 parts by weight of acrylic acid, 1.9 parts by weight of diethyl maleate, 1.4 parts by weight of sodium tripolyphosphate and 200 parts by weight of deionized water were added to the reactor in sequence, and the temperature was heated to 72°C and kept warm for 30 minutes; 5.5 parts by weight of K 2 S 2 O 8 The aqueous solution was kept warm for 30 minutes, and then 3.2 parts by weight of an aqueous solution of mercaptoethanol was uniformly added dropwise to the reactor, and the reaction was continued for 45 minutes; heating was stopped and the mixture was naturally cooled to room temperature, and the pH value of the product was adjusted to 6.8 using a KOH solution.

2. A polycarboxylate water-reducing agent, It is characterized in that The polycarboxylate water reducer is prepared by the method according to claim 1.