A grouting process for repairing leakage in underground concrete retaining structures.

By using drilled holes to bury grouting pipes in the underground engineering concrete envelope, first inject acrylate with a short gel time, and then inject acrylate with a long gel time to form a multiple cross-linked system, solving the problem of the curtain grouting method. The problem of large consumables and high drying shrinkage has achieved low-cost and efficient leakage repair results.

CN117107768BActive Publication Date: 2024-10-22YUNNAN MANZHAO CONSTR ENG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311276088.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-29
Publication Date
2024-10-22
Estimated Expiration
2043-09-29

AI Technical Summary

Technical Problem

Among the existing leakage repair methods for underground engineering concrete envelope structures, the curtain grouting method consumes a large amount of materials, is high in cost, and has a high drying shrinkage rate of the grouting material, which affects the stability of the repair.

Method used

The segmented detachable grouting pipe is buried in the back surface of the concrete envelope by drilling holes. First, acrylate with a short gel time is injected, and then acrylate with a long gel time is injected. A multiple cross-linked system is formed through secondary grouting. , improve anti-dry shrinkage and water retention properties.

Benefits of technology

It significantly reduces the usage of grouting materials, improves construction economy and maintenance stability, forms a sealed flexible waterproof structure, and ensures long-term waterproof performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117107768B_ABST
    Figure CN117107768B_ABST
Patent Text Reader

Abstract

The invention discloses a grouting process for repairing leakage of a concrete enclosure structure of an underground project, comprising the following steps: (1) drilling a hole on the back surface of the concrete enclosure structure, the drilling depth of which is to the thickness of the concrete enclosure wall minus 4-6 mm, and does not penetrate the flexible waterproof layer on the front surface; (2) burying a segmented detachable grouting pipe in the drilled hole; (3) first injecting an acrylate with a short gel time from the grouting pipe, and then injecting an acrylate with a long gel time, until the adjacent grouting holes have grouting back, and then stopping the grouting; after observing for 48 hours, the leakage condition gradually disappears, and the grouting plugging effect is achieved. The process uses less acrylate and has low cost; and through secondary grouting, the leakage repair effect is excellent and the stability is strong.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a concrete structure leakage repair process, in particular to a grouting process for repairing leakage of a concrete enclosure structure of an underground project. Background Art

[0002] Underground construction projects mainly include industrial and civil underground projects, underground subways, municipal tunnels, underground pipelines and other construction projects. Due to the particularity of the location of underground construction projects and the characteristics of the structure itself, after the completion of the project, the building's concrete enclosure structure, such as the bottom plate, side wall, and top plate structure, is difficult to repair and update for self-waterproofing and flexible external waterproofing. Once leakage occurs, leakage repair can generally only be carried out from inside the building.

[0003] At present, the most commonly used method for leakage caused by the damage of the outer flexible waterproofing membrane of the concrete enclosure structure of underground projects and the failure of flexible waterproofing is the curtain grouting method. The curtain grouting method is a widely used plugging and water control measure in engineering. Its construction is to first drill through the concrete enclosure structure, and then inject the quick-setting plugging agent or grouting material through the grouting pipe between the concrete enclosure structure and the original base layer such as the rock and soil layer through the hydraulic or pneumatic method. After solidification, a curtain-like waterproof layer with certain strength and impermeability is formed on the periphery of the building to cut off the water flow, thereby achieving the effect of plugging and waterproofing. However, the main problem of the curtain grouting method is that in order to form the curtain waterproof layer, the amount of grouting material used is too large, the construction time is long, on the one hand, the cost of leakage repair is high, and on the other hand, the large amount of chemical grouting materials used will also cause environmental pollution. Another problem is that the grouting material commonly used for leakage repair is acrylate. After acrylate forms a solid, the shrinkage rate is relatively large, and its shrinkage will directly affect the stability of leakage repair. Summary of the invention

[0004] In view of this, the purpose of the present invention is to provide a grouting process for repairing leakage of concrete retaining structures of underground projects in view of the deficiencies in the prior art, which uses less acrylate and has low cost; and through secondary grouting, the leakage repair effect is excellent and the stability is strong.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A grouting process for repairing leakage of a concrete enclosure structure of an underground project, comprising the following steps:

[0007] (1) Drill holes on the back side of the concrete retaining structure to a depth equal to the thickness of the concrete retaining wall minus 4-6 mm, without penetrating the flexible waterproof layer on the front side;

[0008] (2) Insert a segmented detachable grouting pipe into the drilled hole;

[0009] (3) First inject acrylate with a short gel time from the grouting pipe, then inject acrylate with a long gel time, and stop grouting when grouting returns to the adjacent grouting holes. After observing for 48 hours, the leakage gradually disappears, and the grouting plugging effect is achieved.

[0010] Furthermore, the drill holes in step (1) are distributed in a plum blossom shape, with a hole spacing of 60-70 cm and a hole diameter of 14 mm.

[0011] Furthermore, the acrylate with short gel time has a gel time of 20-30s.

[0012] Furthermore, the concrete enclosure structure is a concrete bottom plate, a concrete side wall, or a concrete top plate.

[0013] Furthermore, the acrylate with a long gel time is prepared by mixing component A and component B in a weight ratio of 1:1, component A: 100 parts of acrylate solution, 5-8 parts of acrylamide, 2-3 parts of N,N-methylenebisacrylamide, 2-3 parts of polyethylene glycol diacrylate, 0.2-0.4 parts of surfactant, 2-3 parts of octadecyl methacrylate, 1-1.5 parts of accelerator, 4-6 parts of montmorillonite, component B: 0.8-1.0 parts of initiator, 10-12 parts of water, and 1-2 parts of silane coupling agent.

[0014] Furthermore, the surfactant is sodium dodecylbenzene sulfonate or fatty alcohol polyoxyethylene ether.

[0015] Furthermore, the acrylate is prepared by mixing magnesium acrylate and calcium acrylate with water in a weight ratio of 2:1, and the concentration of the acrylate solution is 18-22%.

[0016] The beneficial effects of the present invention are:

[0017] 1. The present invention discloses a grouting process for repairing leakage of a concrete enclosure structure of an underground project. First, a hole is drilled on the back surface of the concrete. The drilling depth is about 4-6mm less the thickness of the concrete wall, and the flexible waterproofing on the front surface is not penetrated. Then a grouting pipe is buried, and an acrylate with a short gel time and an acrylate with a long gel time are respectively injected through a secondary composite grouting method. The polyacrylate has low viscosity, good fluidity and permeability, and can quickly penetrate into the concrete wall and between the wall and the flexible waterproofing on the front surface. The acrylate with a short gel time is injected in the initial grouting, which solidifies quickly and can quickly achieve cavity filling and preliminary water-stopping effects, and initially achieves anti-seepage and water-stopping on the front surface of the structure, greatly reducing the high material consumption generated by traditional grouting, and improving the economy of grouting construction.

[0018] Then the secondary grouting is performed to supplement the initial grouting. After the large cavity is initially filled, compensation is performed. The acrylate with a long gel time is used in the secondary grouting of this application, which has certain expansion performance and excellent water retention performance. It is resistant to shrinkage after curing. After the secondary supplementary grouting, it can ensure that the grouting is fully full and dense, forming a complete and closed flexible waterproof structure, thereby achieving excellent waterproof performance. Compared with traditional curtain grouting maintenance, the difficulty of maintenance work is reduced, the fullness of grouting is improved, the amount of grouting material used is small, and the cost is low.

[0019] 2. The present application aims at the main problems of acrylate grouting materials at present, namely, poor water retention performance and relatively large shrinkage rate after forming a solidified product. Therefore, its shrinkage will directly affect the stability of leakage repair. Therefore, the acrylate with a long gel time for the second grouting is improved, wherein octadecyl methacrylate and montmorillonite are added, wherein under the action of a surfactant, octadecyl methacrylate enters the hydrophobic core of the surfactant micelle, and forms a uniform dispersion system with montmorillonite, acrylamide, polyethylene glycol diacrylate and acrylate, and then is initiated by an initiator, wherein acrylate and acrylamide undergo self-polymerization and copolymerization, and the hydrophobic micelles undergo in-situ polymerization, and can also copolymerize with acrylamide; furthermore, the uniformly dispersed montmorillonite enters the montmorillonite interlayer for polymerization through physical adsorption with acrylamide and polyacrylate, forming a multiple cross-linked system with high strength, excellent water retention performance, not easy to lose water, and resistance to shrinkage.

[0020] Furthermore, the hydrophilicity of the gel system of the present application and the hydrophilic effect of montmorillonite enable the acrylate with a long gel time to absorb water and swell. A small amount of cross-linking agent polyethylene glycol diacrylate is also added to the acrylate. The polymer will continue to hydrolyze and break under the action of temperature, pressure, etc., so that the system further absorbs water and swells, increasing the expansibility of the present application and ensuring that the secondary grouting is full and dense. In addition, due to the multiple cross-linking system and hydrophobic chains of the present application, the expansion of the molecular chain is limited, which can reduce shrinkage while ensuring expansion.

[0021] The gel structure has strong self-repairing ability, and the added octadecyl methacrylate molecular chain is flexible. When the gel structure is destroyed, the hydrophobic micelle polymer chain can easily recombine; and the montmorillonite and acrylamide and polyacrylate can also be rebuilt through physical adsorption, ensuring the long-term stability of leakage repair. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a schematic diagram of the implementation state of the present invention;

[0023] Figure 2 Schematic diagram of grouting hole distribution.

[0024] In the figure: 1-decorative layer, 2-leveling layer, 3-concrete wall, 4-flexible waterproof layer. Implementation

[0025] The present invention will be further described below in conjunction with the accompanying drawings and embodiments. Example 1

[0026] A grouting process for repairing leakage of a concrete enclosure structure of an underground project, wherein the concrete enclosure structure is a concrete bottom plate, a concrete side wall, or a concrete top plate. In this embodiment, the concrete enclosure structure of the underground project is a concrete side wall. The basic structure is as follows Figure 1 As shown, from inside to outside, there are a decorative layer 1, a leveling layer 2, a concrete wall 3 and a flexible waterproof layer 4, wherein the leakage caused by the damage and failure of the flexible waterproof layer 4, the specific leakage repair grouting process includes the following steps:

[0027] (1) Drill holes on the back side of the concrete retaining structure. The drilling depth should be about 5 mm less than the thickness of the concrete retaining wall. The flexible waterproof layer 4 on the front side should not be penetrated. The holes should be distributed in a plum blossom shape (e.g. Figure 2 As shown), the hole spacing is 60-70cm, in this embodiment, the hole spacing is 60, and the hole diameter is 14mm;

[0028] (2) embedding a segmented detachable grouting pipe 5 in the drilled hole;

[0029] (3) First, inject acrylate with a short gel time from the grouting pipe. The gel time of acrylate with a short gel time is 20-30s. When the grouting pressure increases from the initial grouting to the stable pressure state of 0.2Mpa to 0.3Mpa, stop grouting. Then continue to inject acrylate with a long gel time until there is grouting back to the adjacent grouting holes. After observing for 48 hours, the leakage gradually disappears, and the grouting plugging effect is achieved.

[0030] Acrylate with short gel time adopts the common two-component acrylate grouting material on the market, and the gel time is about 30 seconds. This embodiment adopts the two-component acrylate grouting material of Oriental Yuhong, and the curing time after the A and B components are mixed is about 30 seconds.

[0031] The acrylate with a long gel time in the present application is prepared by mixing component A and component B in a weight ratio of 1:1, component A: 100 parts of acrylate solution, 5 parts of acrylamide, 2 parts of cross-linking agent N,N-methylenebisacrylamide, 3 parts of polyethylene glycol diacrylate, 0.2 parts of surfactant, 2 parts of octadecyl methacrylate, 1 part of accelerator sodium thiosulfate, 4 parts of montmorillonite, component B: 0.8 parts of initiator ammonium persulfate, 10 parts of water, and 1 part of silane coupling agent.

[0032] The surfactant is sodium dodecylbenzene sulfonate; the acrylate is a mixture of magnesium acrylate and calcium acrylate in a weight ratio of 2:1 with water, and the concentration of the acrylate solution is 18%. Example 2

[0033] The difference between Example 2 and Example 1 is that:

[0034] The acrylate with a long gel time in the present application is prepared by mixing component A and component B in a weight ratio of 1:1, component A: 100 parts of acrylate solution, 6 parts of acrylamide, 2.5 parts of crosslinking agent N,N-methylenebisacrylamide, 2.8 parts of polyethylene glycol diacrylate, 0.3 parts of surfactant, 2.5 parts of octadecyl methacrylate, 1.2 parts of accelerator sodium thiosulfate, 4.5 parts of montmorillonite, component B: 0.8 parts of initiator ammonium persulfate, 11 parts of water, and 1.2 parts of silane coupling agent.

[0035] The surfactant is sodium dodecylbenzene sulfonate; the acrylate is a mixture of magnesium acrylate and calcium acrylate in a weight ratio of 2:1 with water, and the concentration of the acrylate solution is 20%. Example 3

[0036] The difference between Example 3 and Example 1 is that:

[0037] The acrylate with a long gel time in the present application is prepared by mixing component A and component B in a weight ratio of 1:1, component A: 100 parts of acrylate solution, 7 parts of acrylamide, 2.8 parts of crosslinking agent N,N-methylenebisacrylamide, 2.5 parts of polyethylene glycol diacrylate, 0.35 parts of surfactant, 2.5 parts of octadecyl methacrylate, 1.4 parts of accelerator sodium thiosulfate, 5 parts of montmorillonite, component B: 1.0 parts of initiator ammonium persulfate, 11.5 parts of water, and 1.5 parts of silane coupling agent.

[0038] The surfactant is sodium dodecylbenzene sulfonate; the acrylate is a mixture of magnesium acrylate and calcium acrylate in a weight ratio of 2:1 with water, and the concentration of the acrylate solution is 20%. Example 4

[0039] The difference between Example 4 and Example 1 is that:

[0040] The acrylate with a long gel time in the present application is prepared by mixing component A and component B in a weight ratio of 1:1, component A: 100 parts of acrylate solution, 8 parts of acrylamide, 3 parts of cross-linking agent N,N-methylenebisacrylamide, 2 parts of polyethylene glycol diacrylate, 0.4 parts of surfactant, 3 parts of octadecyl methacrylate, 1.5 parts of accelerator sodium thiosulfate, 6 parts of montmorillonite, component B: 0.9 parts of initiator ammonium persulfate, 12 parts of water, and 2 parts of silane coupling agent.

[0041] The surfactant is sodium dodecylbenzene sulfonate; the acrylate is a mixture of magnesium acrylate and calcium acrylate in a weight ratio of 2:1 with water, and the concentration of the acrylate solution is 20%.

[0042] Comparative Example 1

[0043] Comparative Example 1 is a comparative example of Example 4, and is different from Example 4 in that acrylamide and octadecyl methacrylate are not added, specifically:

[0044] Component A: 100 parts of acrylate solution, 3 parts of crosslinking agent N,N-methylenebisacrylamide, 2 parts of polyethylene glycol diacrylate, 0.4 parts of surfactant, 1.5 parts of accelerator sodium thiosulfate, 6 parts of montmorillonite, component B: 1.0 parts of initiator ammonium persulfate, 12 parts of water, 2 parts of silane coupling agent.

[0045] Application test

[0046] By adopting the secondary grouting process in Example 1, the effective expansion radius of a single hole is about 80 cm, and the effective grouting range is about 2 square meters. According to the average porosity of the wall membrane and the structure of 3 mm, the acrylate consumption of the first grouting of a single hole can be controlled within the range of 6 kg, and the secondary grouting consumption can be controlled within the range of 2 kg. Compared with the traditional wall grouting with a single hole consumption of 40 to 50 kilograms, the economy is much improved. In addition, after the secondary grouting, the gel has high water retention, anti-shrinkage, and very stable performance. It can be stably maintained for more than 5 years after leakage repair.

[0047] Performance testing of acrylates with long gel times

[0048] The gel time, expansion performance, elongation at break and volume shrinkage of the acrylic acid salts with long gel time prepared in Examples 1 to 4 of the present application and Comparative Example 1 were tested.

[0049] Elongation at break: Two 40mm×20mm×10mm standard mortar blocks are placed in a silicone mold with a cavity size of 100mm×20mm×10mm to form a 20mm×20mm×10mm cavity in the middle, and the acrylate with a long gel time prepared in Examples 1-4 of the present application and Comparative Example 1 is cast. After gelation, it is covered with plastic wrap to prevent the evaporation of water in the gel. After 1 day, the mortar blocks are demolded to obtain a tensile specimen. A tensile test is performed using a micro-controlled electronic universal testing machine. The elongation when the gel breaks or debonds from the standard mortar block is the elongation at break.

[0050] Swelling performance: The swelling performance of gel is measured by pouring 20ml of slurry into a 50ml beaker to generate the gel as a test piece. First, measure its diameter and height, convert it into volume, and then put it into water to allow it to swell freely. Regularly test its volume change until it stops swelling. There are 3 test pieces in each group, and the test results are calculated according to the following formula to calculate the swelling ratio: Swelling ratio = volume of the test piece after swelling / volume of the test piece before swelling * 100%.

[0051] Test method for volume shrinkage of gel after water loss: acrylate is made into a gel sample of 20 mm × 20 mm × 10 mm in size to obtain the initial volume of the gel. The size of the sample is then measured after drying for a certain period of time in an environment of (23 ± 2) ° C and humidity of (50 ± 10)%, and the volume of the gel after drying is obtained. The volume shrinkage is calculated. The test results are shown in Table 1.

[0052] Table 1 Performance test data

[0053]

[0054] The acrylate with a long gel time prepared in Examples 1-4 of the present application has a gel time of 290-386s, strong flexibility, certain water absorption and expansion properties, and a very low volume shrinkage rate after drying. It has strong anti-shrinkage performance and can greatly enhance the stability of leak repair.

[0055] Comparative Example 1 is a comparative example of Example 4. No acrylamide and octadecyl methacrylate are added to the raw materials. Combined with the test data, it can be seen that its expansion rate is slightly higher than that of Example 4, but its flexibility and anti-shrinkage performance are much lower than those of Example 4, indicating that the multiple gel system of the present application can increase the flexibility and anti-shrinkage performance of the gel.

[0056] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Other modifications or equivalent substitutions made to the technical solution of the present invention by ordinary technicians in the field should be included in the scope of the claims of the present invention as long as they do not depart from the spirit and scope of the technical solution of the present invention.

Claims

1. A grouting process for repairing leakage of concrete enclosure structure of underground engineering, characterized by: The following steps are involved: (1) Drill holes on the back side of the concrete retaining structure to a depth equal to the thickness of the concrete retaining wall minus 4-6 mm, without penetrating the flexible waterproof layer on the front side; (2) Insert a segmented detachable grouting pipe into the drilled hole; (3) First inject acrylate with a short gel time from the grouting pipe, then inject acrylate with a long gel time. Stop grouting when grouting returns to the adjacent grouting holes and observe for 48 hours. The drill holes in step (1) are distributed in a plum blossom shape, with a hole spacing of 60-70 cm and a hole diameter of 14 mm; The acrylate with a long gel time is prepared by mixing component A and component B in a weight ratio of 1:

1. Component A includes 100 parts of acrylate solution, 5-8 parts of acrylamide, 2-3 parts of N,N-methylenebisacrylamide, 2-3 parts of polyethylene glycol diacrylate, 0.2-0.4 parts of surfactant, 2-3 parts of octadecyl methacrylate, 1-1.5 parts of accelerator and 4-6 parts of montmorillonite. Component B includes 0.8-1.0 parts of initiator, 10-12 parts of water and 1-2 parts of silane coupling agent.

2. The grouting process for repairing leakage of concrete enclosure structure of underground engineering according to claim 1 is characterized by: The acrylate with short gel time has a gel time of 20-30s.

3. The grouting process for repairing leakage of concrete enclosure structure of underground engineering according to claim 1 is characterized by: The concrete enclosure structure is a concrete bottom plate, a concrete side wall or a concrete top plate.

4. The grouting process for repairing leakage of concrete enclosure structure of underground engineering according to claim 1 is characterized by: The surfactant is sodium dodecylbenzene sulfonate or fatty alcohol polyoxyethylene ether.

5. The grouting process for repairing leakage of concrete enclosure structure of underground engineering according to claim 1 is characterized by: The acrylate solution is prepared by mixing magnesium acrylate and calcium acrylate with water in a weight ratio of 2:1, and the concentration of the acrylate solution is 18-22%.