A Zn-doped sodium ion layered oxide and its preparation method and application

The Zn doping method solves the problem of performance attenuation of sodium ion layered oxide during the discharge process, improves its electrochemical stability and cycle performance, and is suitable for high-performance sodium ion battery cathode materials.

CN117133898BActive Publication Date: 2024-10-15QILU UNIVERSITY OF TECHNOLOGY (SHANDONG ACADEMY OF SCIENCES)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311172266.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-12
Publication Date
2024-10-15
Estimated Expiration
2043-09-12

AI Technical Summary

Technical Problem

The Ginger Taylor effect and phase change of Mn3+ occur during the discharge process of sodium ion layered oxide, resulting in battery capacity attenuation, and its air stability is poor, and it easily reacts with water and carbon dioxide in the air, exacerbating the attenuation of battery performance. Solid-phase method The loss of sodium source and too small grain size during preparation also affect the performance of the battery core.

Method used

Using the Zn doping method, zinc oxide or zinc nitrate is incorporated into the sodium ion layered oxide precursor, and the volatilization loss of the Na source is suppressed through high-temperature crystal growth, forming a pure phase sodium ion layered oxide with larger particle size. Used as cathode material for sodium-ion batteries.

Benefits of technology

It effectively suppresses the performance attenuation of sodium ion layered oxide, improves electrochemical stability and cycle performance, and ensures high cycle times and capacity retention rate of the battery in the voltage range of 2.0-4.0 V.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117133898B_ABST
    Figure CN117133898B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of crystal growth and battery material preparation, and in particular relates to a Zn-doped sodium ion layered oxide and its preparation method and application. The general structural formula of the sodium ion layered oxide is NaNi i Fe j Mn k O2, wherein i+j+k=1; the Zn-doped sodium ion layered oxide is a pure phase sodium ion layered oxide, and Zn is doped into the crystal lattice of the sodium ion layered oxide; the particle size of the Zn-doped sodium ion layered oxide is 3 to 8 um. The present invention incorporates a dopant such as zinc oxide or zinc nitrate that does not introduce impurity elements into a sodium ion layered oxide precursor, and Zn inhibits the volatilization loss of the Na source during crystal growth. The present invention can effectively inhibit the volatilization loss of the Na source during the growth of the sodium ion layered oxide crystal by Zn doping, thereby avoiding excessive sodium source. At the same time, the fluxing effect of the Zn element at high temperature enables the sodium ion layered oxide crystal to grow into a single crystal with a larger particle size, thereby improving its electrochemical stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of crystal growth and battery material preparation, and in particular relates to a Zn-doped sodium ion layered oxide and a preparation method and application thereof. Background Art

[0002] Sodium ion layered oxide is a crystalline material made of sodium, nickel, cobalt, manganese and other metal elements in a certain ratio. Due to its low cost, low toxicity and high theoretical specific capacity, it has become one of the potential candidate materials for the positive electrode of sodium ion batteries and has attracted great interest from researchers. However, at the end of the discharge process, this material will have Mn 3+ The Jan-Taylor effect and phase change cause the battery capacity to decay during the charge and discharge process. Secondly, layered metal oxides have poor air stability and are easily reacted with water and carbon dioxide in the air to promote the formation of alkaline substances, which also aggravates the performance decay of the battery cell. In addition, when sodium ion layered oxides are prepared by the solid phase method, the sodium source is lost at high temperatures and an excessive amount of sodium source is required, which also causes an increase in the residual alkali content and accelerates the performance decay of the battery cell. At the same time, the small grains of sodium ion layered oxides prepared by the solid phase method (less than 2 um) will also cause the performance decay of the battery cell.

[0003] In order to suppress the performance degradation of sodium ion layered oxides, coating and doping methods are usually used in the prior art to modify them. However, the coating and doping modification methods in the prior art have the following disadvantages: (1) Although the currently reported methods of coating sodium ion layered oxides with oxides and polymers can slow down the corrosion of electrolytes through a physical protective layer, they have problems such as reduced energy density and reduced electrolyte compatibility, which affect battery performance; (2) Although doping modification can improve the performance of sodium ion layered oxides, it is difficult to solve the problem of residual alkali due to excessive sodium carbonate, which aggravates the performance degradation of the battery cell. Summary of the invention

[0004] In view of the problems of sodium source loss and small grain size (less than 2 um) of sodium ion layered oxide when preparing sodium ion layered oxide by solid phase method, the present invention provides a Zn-doped sodium ion layered oxide and its preparation method and application. In the present invention, a dopant such as zinc oxide or zinc nitrate that does not introduce impurity elements is added to the sodium ion layered oxide precursor, and Zn can inhibit the volatilization loss of the Na source during crystal growth.

[0005] To achieve the above object, the present invention adopts the following technical solution:

[0006] One of the purposes of the present invention is to provide a Zn-doped sodium ion layered oxide, the general structural formula of which is NaNi i Fe j Mn kO2, wherein i+j+k=1; the Zn-doped sodium ion layered oxide is a pure phase sodium ion layered oxide, and Zn is doped into the lattice of the sodium ion layered oxide; the particle size of the Zn-doped sodium ion layered oxide is 3 to 8 um.

[0007] The second object of the present invention is to provide a method for preparing the above-mentioned Zn-doped sodium ion layered oxide, comprising the following steps:

[0008] (1) ball milling a Na source, a Ni source, a Fe source, a Mn source and a Zn source according to a stoichiometric ratio to prepare a precursor;

[0009] (2) The precursor in step (1) is placed in a tube furnace, and the temperature is raised from 25°C to 800-1100°C. After being kept at this temperature for a period of time, the precursor is cooled in the furnace to obtain a Zn-doped sodium ion layered oxide.

[0010] According to the preferred embodiment of the present invention, the molar ratio of the Ni source, Fe source, Mn source and Na source in step (1) satisfies NaNi i Fe j Mn k O2, i+j+k=1.

[0011] According to the preferred embodiment of the present invention, the Na source in step (1) is sodium carbonate or sodium nitrate. The Na source is a raw material that does not introduce impurity elements when the sodium ion layered oxide crystal phase is formed.

[0012] Preferably, according to the present invention, the Na source in step (1) is weighed strictly according to the chemical ratio without any excess or deficiency.

[0013] Preferably, according to the present invention, the Ni source in step (1) is a combination of one or more of NiO, Ni2O3 or Ni(NO3)2·6H2O.

[0014] Preferably, according to the present invention, the Fe source in step (1) is one or more combinations of Fe2O3, Fe2O3, Fe3O4, or Fe(NO3)3·9H2O.

[0015] Preferably, according to the present invention, the Mn source in step (1) is a combination of one or more of MnO2, Mn2O3, and MnO.

[0016] According to the preferred embodiment of the present invention, the Zn source in step (1) is ZnO or Zn(NO3)2·6H2O. The Zn source is a Zn-containing raw material without introducing impurity elements, and the amount used is Na:Zn=1mol:xmol, x=0.001-0.015.

[0017] Preferably, according to the present invention, the tubular furnace in step (2) is an air-circulating tubular furnace.

[0018] Preferably, according to the present invention, the programmed heating rate in step (2) is 2 to 10° C. / min.

[0019] Preferably, according to the present invention, the insulation time in step (2) is 18 to 30 h.

[0020] The third object of the present invention is to disclose the application of the above-mentioned Zn-doped sodium ion layered oxide, wherein the Zn-doped sodium ion layered oxide is used as a positive electrode active material for a sodium ion battery.

[0021] Beneficial Effects

[0022] The invention discloses a Zn-doped sodium ion layered oxide. The invention can effectively suppress the volatilization loss of the Na source during the growth of the sodium ion layered oxide crystal by Zn doping, thereby avoiding the increase of the residual alkali content caused by excessive use of the sodium source. At the same time, the fluxing effect of the Zn element at high temperature enables the sodium ion layered oxide crystal to grow into a single crystal with a larger particle size, thereby improving its electrochemical stability. The theoretical basis and technical support are provided for the production of high-performance sodium ion layered oxide positive electrode materials.

[0023] The Zn-doped sodium ion layered oxide prepared by the method of the present invention is a pure phase sodium ion layered oxide, indicating that Zn is doped into its lattice. The particle size of the Zn-doped sodium ion layered oxide is 3 to 8 um, and single crystals with larger particle sizes are conducive to improving cycle performance.

[0024] The Zn-doped sodium ion layered oxide obtained by the inventive method is used as a positive electrode active material in a sodium ion battery. The electrochemical cycle curve is tested. Within the voltage range of 2.0-4.0 V, it can be stably cycled for more than 2000 times at a rate of 0.1 C, and the capacity retention rate is more than 80%. The increase in the particle size of the sodium ion layered oxide and the solution to the problem of excessive sodium source usage achieve an improvement in the cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The zinc-doped NaNi prepared in Example 1 of the present invention 1 / 3 Fe 1 / 3 Mn 1 / 3 X-ray powder diffraction pattern of O2;

[0026] Figure 2 The zinc-doped NaNi prepared in Example 1 of the present invention 1 / 3 Fe 1 / 3 Mn 1 / 3 Scanning electron microscope image of O2;

[0027] Figure 3 The zinc-doped NaNi prepared in Example 1 of the present invention 1 / 3 Fe 1 / 3 Mn 1 / 3 Electrochemical cycle curve of O2. DETAILED DESCRIPTION

[0028] Hereinafter, the present invention will be described in detail. Before describing, it should be understood that the terms used in this specification and the appended claims should not be interpreted as being limited to the general meaning and dictionary meaning, but should be interpreted according to the meaning and concept corresponding to the technical aspects of the present invention on the basis of the principle that the inventor is allowed to appropriately define the terms for the best interpretation. Therefore, the descriptions presented here are only preferred examples for illustrative purposes and are not intended to limit the scope of the present invention, so that it should be understood that other equivalents or improvements can be obtained therefrom without departing from the spirit and scope of the present invention.

[0029] The following examples are only listed as examples of embodiments of the present invention and do not constitute any limitation to the present invention. It can be understood by those skilled in the art that modifications within the scope of the essence and concept of the present invention fall within the scope of protection of the present invention. Unless otherwise specified, the reagents and instruments used in the following examples are commercially available products.

[0030] Terminology

[0031] Zn doping: doping with zinc oxide or zinc nitrate, which does not introduce impurity elements, into the sodium ion layered oxide precursor. Zn inhibits the volatilization loss of the Na source during crystal growth.

[0032] The raw materials used in the examples and comparative examples are all conventional raw materials.

[0033] Example 1

[0034] A Zn-doped sodium ion layered oxide comprises the following steps:

[0035] (1) Na2CO3, NiO, Fe2O3, MnO2 and ZnO were weighed in a molar ratio of 1 / 2:1 / 3:1 / 6:1 / 3:1 / 600 and ball-milled for 12 h to prepare a precursor;

[0036] (2) The precursor in step (1) was placed in a tube furnace, and the temperature was raised from 25 °C to 900 °C. After being kept at this temperature for 24 h, the precursor was cooled in the furnace to obtain Zn-doped NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2.

[0037] The obtained sample - Zn-doped NaNi 1 / 3Fe 1 / 3 Mn 1 / 3 X-ray powder diffraction of O2 Figure 1 As shown. Figure 1 The analysis shows that pure NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2, indicating that Zn is incorporated into its lattice.

[0038] The Zn-doped NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 The sample size of O2 is as follows Figure 2 As shown. Figure 2 The analysis shows that the Zn-doped NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 The O2 particles are uniform in size, about 3 um.

[0039] The Zn-doped NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2 is used as the positive electrode active material in sodium ion batteries. Its electrochemical cycle curve is as follows: Figure 3 As shown. Figure 3 Analysis shows that within the voltage range of 2.0-4.0 V, it can be stably cycled for more than 2000 times at a rate of 0.1 C, with a discharge capacity of 140.7 mAh / g and a capacity retention rate of 84.3%.

[0040] Example 2

[0041] A Zn-doped sodium ion layered oxide comprises the following steps:

[0042] (1) Na2CO3, NiO, Fe2O3, MnO2 and ZnO were weighed in a molar ratio of 0.5:0.3:0.25:0.2:0.001 and ball-milled for 12 h to prepare a precursor;

[0043] (2) The precursor in step (1) was placed in a tube furnace, and the temperature was raised from 25 °C to 900 °C. After being kept at this temperature for 24 h, the precursor was cooled in the furnace to obtain Zn-doped NaNi 0.3 Fe 0.5 Mn 0.2 O2.

[0044] The sample obtained in this example, Zn-doped NaNi 0.3 Fe 0.5 Mn 0.2O2 is used as the positive electrode active material in sodium ion batteries, with a capacity retention rate of 82.6% after 1000 cycles at a rate of 0.1 C in the voltage range of 2.0-4.0 V.

[0045] Example 3

[0046] A Zn-doped sodium ion layered oxide comprises the following steps:

[0047] (1) Na2CO3, NiO, Fe2O3, MnO2 and ZnO were weighed in a molar ratio of 1 / 2:1 / 3:1 / 6:1 / 3:1 / 300 and ball-milled for 12 h to prepare a precursor;

[0048] (2) The precursor in step (1) was placed in a tube furnace, and the temperature was raised from 25 °C to 800 °C. After being kept at this temperature for 24 h, the precursor was cooled in the furnace to obtain Zn-doped NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2.

[0049] The sample obtained in this example, Zn-doped NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2 is used as the positive electrode active material in sodium ion batteries, with a capacity retention rate of 80.9% after 1000 cycles at a rate of 0.1 C in the voltage range of 2.0-4.0 V.

[0050] Example 4

[0051] A Zn-doped sodium ion layered oxide comprises the following steps:

[0052] (1) NaNO3, NiO, Fe2O3, MnO2 and ZnO were weighed in a molar ratio of 1:1 / 3:1 / 6:1 / 3:1 / 600 and ball-milled for 12 h to prepare a precursor;

[0053] (2) The precursor in step (1) was placed in a tube furnace, and the temperature was raised from 25°C to 1000°C. After being kept at this temperature for 24 h, the precursor was cooled in the furnace to obtain Zn-doped NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2.

[0054] The sample obtained in this example, Zn-doped NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2 is used as the positive electrode active material in sodium ion batteries, with a capacity retention rate of 83.5% after 1000 cycles at a rate of 0.1 C in the voltage range of 2.0-4.0 V.

[0055] Example 5

[0056] A Zn-doped sodium ion layered oxide comprises the following steps:

[0057] (1) NaNO3, NiO, Fe2O3, MnO2 and Zn(NO3)2·6H2O were weighed in a molar ratio of 1:1 / 3:1 / 6:1 / 3:3 / 200 and ball-milled for 12 h to prepare a precursor;

[0058] (2) The precursor in step (1) was placed in a tube furnace, and the temperature was raised from 25 °C to 800 °C. After being kept at this temperature for 24 h, the precursor was cooled in the furnace to obtain Zn-doped NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2.

[0059] The sample obtained in this example, Zn-doped NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2 is used as the positive electrode active material in sodium ion batteries, with a capacity retention rate of 81.3% after 1000 cycles at 0.1 C rate in the voltage range of 2.0-4.0 V.

[0060] Comparative Example 1

[0061] Na2CO3, NiO, Fe2O3, and MnO2 were weighed and mixed in a molar ratio of 3:2:2:2 and ball-milled for 12 h to obtain a precursor. The precursor was placed in a tube furnace and heated from 25 °C to 900 °C. After keeping the temperature for 24 h, the precursor was cooled with the furnace to obtain NaNi 1 / 3Fe 1 / 3 Mn 1 / 3 O2.

[0062] The sample obtained in this comparative example - NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2 is used as the positive electrode active material in sodium ion batteries. It can be stably cycled 500 times at a rate of 0.1 C in the voltage range of 2.0-4.0 V with a capacity retention rate of 67.5%.

[0063] Comparative Example 2

[0064] Na2CO3, NiO, Fe2O3, and MnO2 were weighed in a molar ratio of 5:3:5:2 and ball-milled for 12 h to obtain a precursor. The precursor was placed in a tube furnace and heated from 25 °C to 900 °C. After keeping the temperature for 24 h, the precursor was cooled with the furnace to obtain NaNi 0.3 Fe 0.5 Mn 0.2O2.

[0065] The sample obtained in this comparative example - NaNi 0.3 Fe 0.5 Mn 0.2 O2 is used as the positive electrode active material in sodium ion batteries, with a capacity retention rate of 71.6% after 1000 cycles at 0.1 C rate in the voltage range of 2.0-4.0 V.

[0066] By comparing the samples obtained in Examples 1-3 with those obtained in Comparative Examples 1-2, the following conclusion can be drawn: zinc doping can effectively improve the cycle stability of sodium ion layered oxide positive electrode materials.

[0067] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for a person skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to replace some of the technical features therein by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions claimed to be protected by the present invention.

Claims

1. A Zn-doped sodium ion layered oxide, characterized in that: The general structural formula of the sodium ion layered oxide is NaNi i Fe j Mn k O2, wherein i+j+k=1; the Zn-doped sodium ion layered oxide is a pure phase sodium ion layered oxide, and Zn is doped into the lattice of the sodium ion layered oxide; The particle size of the Zn-doped sodium ion layered oxide is 3 to 8 um. The preparation method of the Zn-doped sodium ion layered oxide comprises the following steps: (1) According to the stoichiometric ratio, a Na source, a Ni source, a Fe source, a Mn source and a Zn source are ball-milled and mixed to prepare a precursor; the Na source is sodium carbonate or sodium nitrate, which is weighed strictly according to the stoichiometric ratio without any excess or deficiency; the Zn source is ZnO or Zn(NO3)2·6H2O, and the amount is Na:Zn=1mol:xmol, x=0.001-0.015; (2) The precursor in step (1) is placed in a tube furnace, and the temperature is raised from 25°C to 800-1100°C. After being kept at this temperature for a period of time, the precursor is cooled in the furnace to obtain a Zn-doped sodium ion layered oxide.

2. The sodium ion layered oxide according to claim 1, characterized in that The Ni source in step (1) is one or more of NiO, Ni2O3 or Ni(NO3)2·6H2O.

3. The sodium ion layered oxide according to claim 1, characterized in that The Fe source in step (1) is one or more combinations of Fe2O3, Fe2O3, Fe3O4, or Fe(NO3)3·9H2O.

4. The sodium ion layered oxide according to claim 1, characterized in that The Mn source in step (1) is one or more combinations of MnO2, Mn2O3, and MnO.

5. The sodium ion layered oxide according to claim 1, characterized in that The tubular furnace described in step (2) is an air-circulating tubular furnace.

6. The sodium ion layered oxide according to claim 1, characterized in that The programmed heating rate in step (2) is 2 to 10°C / min; the holding time is 18 to 30 h.

7. The use of the Zn-doped sodium ion layered oxide according to claim 1, characterized in that: The Zn-doped sodium ion layered oxide is used for positive electrode active materials of sodium ion batteries.