Electroluminescent materials of metal organic framework-enriched boron nitride quantum dots and sensors prepared therefrom
By encapsulating boron nitride quantum dots in metal organic frameworks, using hydrothermal synthesis and layer-by-layer self-assembly technology, the problems of complex preparation of traditional boron nitride quantum dots and low ECL efficiency are solved, and high sensitivity and stable electrical Chemiluminescence detection.
Patent Information
- Application Number
- CN202310895624.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-20
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-07-20
AI Technical Summary
The preparation of traditional boron nitride quantum dots is complex and the ECL efficiency is low, resulting in insufficient electrochemiluminescence signals, limiting the application of ECL imaging and molecular detection.
The high quantum yield of hydroxy and amino functionalized boron nitride quantum dots were prepared by simple hydrothermal synthesis method, and encapsulated in a metal organic framework (Zr-MOF), and electroluminescent materials were prepared by layer-layer self-assembly technology. , enhance ECL emission performance.
Improve the intensity and stability of the electrochemiluminescence signal, enhance the detection sensitivity, and realize quantitative detection of tranbolon in ambient water, with high sensitivity, wide linear range, low detection limit, simple operation and good reproducibility .
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electroluminescence, and in particular relates to an electroluminescent material of metal organic framework-enriched boron nitride quantum dots and a sensor prepared therefrom. Background Art
[0002] Electrochemiluminescence (ECL) is an analytical technique that uses electrochemical methods as a means of stimulation to induce chemiluminescence. Due to its many advantages such as low background, high sensitivity, simple equipment and controllable potential, ECL has become one of the research areas that analytical chemists focus on.
[0003] Electrochemiluminescence sensors have both the controllability of chemiluminescence technology and the sensitivity of electrochemical technology. Compared with traditional analytical methods, they have the advantages of high sensitivity, good selectivity, simple operation, and low background signal. Summary of the invention
[0004] The present invention provides an electroluminescent material of metal organic framework enriched boron nitride quantum dots and a sensor prepared therefrom. The material exhibits excellent electroluminescent performance. The electroluminescent sensor prepared therefrom has the advantages of high sensitivity, good selectivity, simple operation, low background signal, etc.
[0005] The technical solution of the present invention is an electroluminescent material with a metal organic framework enriched with boron nitride quantum dots, denoted as BNQDs@MOF, wherein the metal organic framework is a Zr-MOF nanomaterial, and the mass ratio of the Zr-MOF nanomaterial to the boron nitride quantum dots is 1:0.8-1.2.
[0006] Furthermore, when preparing Zr-MOF nanomaterials, BPDC is used as an organic ligand precursor and ZrCl4 is used as a metal precursor. The two are dispersed in a solution and mixed, and acetic acid is added and heated to react. After the reaction, centrifugation, washing and drying are performed to obtain the obtained material.
[0007] Furthermore, when preparing boron nitride quantum dots, HBO3 and ammonia water are used as raw materials, the pH is adjusted to neutral after heating reaction, and centrifugal separation is performed to obtain the boron nitride quantum dots.
[0008] Furthermore, when preparing the electroluminescent material of metal organic framework enriched boron nitride quantum dots, the Zr-MOF nanomaterial is dispersed with ethanol, the carboxyl group is activated by 20 mM EDC and 10 mM NHS, the boron nitride quantum dots are dispersed with ultrapure water, and then the two are mixed in proportion, the solution is stirred at 90-100°C for 12-18 hours, and after centrifugation, it is washed with ethanol and ultrapure water respectively to obtain BNQDs@MOF.
[0009] The present invention also relates to an electrochemiluminescent sensor prepared from the electroluminescent material, the preparation of which comprises the following steps:
[0010] S1. Polish the glassy carbon electrode with alumina and clean it; then place it in p-aminobenzoic acid buffer for electropolymerization, clean and dry it; then use a mixed solution of EDC and NHS to drip onto the electrode surface for treatment, and finally clean and dry it;
[0011] S2, dripping the capture antibody of the object to be detected onto the electrode surface obtained in S1, drying, then dripping bovine serum albumin solution onto the electrode surface to block the non-specific active sites on the electrode surface, washing and drying; dripping a series of antigen solutions of the object to be detected with different concentrations onto the electrode surface, washing and drying again;
[0012] S3, prepare BNQDs@MOF dispersion, add the detection antibody of the object to be detected and mix at room temperature for 4-6 hours, then disperse into the buffer after centrifugation to prepare the detection antibody solution of the object to be detected labeled with BNQDs@MOF;
[0013] S4. Drop the BNQDs@MOF-labeled analyte detection antibody solution obtained in S3 onto the electrode obtained in S2, incubate at room temperature and then wash to obtain an electrochemiluminescent sensor based on metal organic framework-enriched boron nitride quantum dots.
[0014] Furthermore, the glassy carbon electrode in S1 was polished with aluminum oxide particles from coarse to fine in sequence until the surface was a mirror surface, and then cleaned with anhydrous ethanol and ultrapure water in sequence.
[0015] Furthermore, the p-aminobenzoic acid buffer in S1 was mixed with 3.0~7.0mmol / L p-aminobenzoic acid solution and PBS buffer solution. During treatment, the electrode was placed in the mixed solution and scanned at 0.40~1.20V for 3 cycles at a speed of 10mV / s to fix p-aminobenzoic acid to the electrode surface, rinsed with ultrapure water, and dried at room temperature. During EDC and NHS treatment, a mixed solution of 20 mg / mL EDC and 10 mg / mL NHS was added dropwise to the electrode surface, incubated at 35~38℃ for 1~1.5h, rinsed the electrode surface with phosphate buffer, and dried at room temperature.
[0016] Furthermore, the concentration of the capture antibody of the analyte in S2 is 5.0~15.0µg / mL; the concentration of the bovine serum albumin solution is 0.8~1.2mg / mL; a series of different concentrations of the analyte antigen solution are between 0.0001~40ng / mL; phosphate buffer is used for washing in S2, and it is dried in a refrigerator at 4°C.
[0017] Furthermore, in S3, BNQDs@MOF was dispersed in ultrapure water at a concentration of 2 mg / mL, and the concentration of the analyte detection antibody was 8~12 µM; in S4, the concentration of the analyte detection antibody solution labeled with BNQDs@MOF was 1.0~3.0 mg / mL.
[0018] Furthermore, the analyte is trenbolone (TBE).
[0019] Traditional boron nitride quantum dots have the fatal defects of complex preparation and extremely low ECL efficiency, which leads to limitations in the fields of ECL imaging, molecular detection and optical devices. The boron nitride quantum dots prepared by a simple hydrothermal synthesis method in the present invention have high ECL efficiency, excellent biocompatibility and low toxicity as ECL emitters. Specifically, high quantum yield hydroxyl and amino functionalized boron nitride quantum dots (BNQD) are synthesized through an aqueous route. The method adopts a bottom-up approach to hydrothermally treat a mixture of boric acid and ammonia solution. The functionalized BNQDs have excellent luminescent properties and can be easily dispersed in an aqueous medium. The method has the advantages of cheap raw materials, large synthesis quality, environmental friendliness, high dispersibility, high quantum yield (QY), strong fluorescence, and large Stokes shift.
[0020] Compared with free BNQDs in solution, nanoreactor MOF can confine BNQDs to a narrow area to increase the collision frequency between reactants, thereby significantly improving the reaction efficiency. The nanoscale confined space can provide a suitable reaction microenvironment for enhancing ECL emission. Specifically, the confined and stable porous structure increases the accumulation of intermediate radicals and co-reactants to enhance electron / proton transfer. Therefore, nanoreactors can be used to constrain enhanced ECL and improve detection sensitivity.
[0021] The present invention has the following beneficial effects:
[0022] 1. The metal-organic framework (MOFs) in the present invention is a porous hybrid material with a periodic network structure composed of a metal center and an organic ligand, which has a high specific surface area, a high porosity structure, adjustable pore size, unsaturated metal sites, structural flexibility and excellent optical properties. Boron nitride quantum dots (BNQDs) are encapsulated into MOF. The porous structure and high specific surface area of MOF can not only increase the load of BNQDs and improve the ECL intensity; they can also act as a reliable barrier to protect the boron nitride quantum dots from the external environment and prevent the leakage of BNQDs, thereby improving the stability of the ECL signal. The composite material provides a confined structure, and the boron nitride quantum dots (BNQDs) are embedded in the MOF composite (BNQDs@MOF), which solves the problem of low electrochemiluminescence signal and exhibits enhanced electrochemiluminescence emission performance.
[0023] 2. The present invention utilizes layer-by-layer self-assembly technology to prepare an immunosensor based on the luminescence of metal organic framework-enriched boron nitride quantum dots, using p-aminobenzoic acid as a substrate to fix antibodies; at the same time, potassium persulfate is used as a co-reactant to promote the generation of excited states of the metal organic framework-enriched boron nitride quantum dot composite material, thereby enhancing the electrochemiluminescence efficiency, increasing the signal change value during the test, and improving the sensitivity of the detection.
[0024] 3. The sensor provided by the present invention can be used to quantitatively detect trenbolone in environmental water, and has the advantages of wide linear range, low detection limit, high sensitivity, simple operation, fast detection speed, etc. It also has good reproducibility, stability and selectivity, and can achieve specific detection. DETAILED DESCRIPTION
[0025] The embodiments of the present invention will be described in detail below with reference to examples, but those skilled in the art will appreciate that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention.
[0026] Example 1
[0027] The electroluminescent material of metal organic framework enriched boron nitride quantum dots comprises the following steps during preparation:
[0028] (1) Preparation of Boron Nitride Quantum Dots (BNQDs)
[0029] 0.8 g HBO3 was added to 30 ml ultrapure water and ultrasonicated for 5 min to obtain a homogeneous solution. Then 2.4 mL concentrated ammonia was added and stirred evenly. The obtained solution was transferred to an autoclave and heated to 200 °C for 12 h to obtain a uniform and transparent solution. The pH value was adjusted to 7.0 with 0.1 M HCl. After centrifugation, the obtained product was dispersed in water and stored in a refrigerator at 4 °C for later use.
[0030] (2) Preparation of BNQDs@MOF
[0031] 40 mg BPDC was dispersed in DMF containing 360 μL triethylamine as an organic ligand precursor solution. 45 mg ZrCl4 was ultrasonically dispersed in 16 mL DMF as a white metal precursor solution. Then, the two solutions were mixed with 2.25 mL acetic acid, transferred to a Teflon-sealed autoclave for high-pressure reaction, and left to stand at 90 °C for 24 h. After the solvothermal reaction, it was centrifuged at 6500 rpm for 12 min and then washed with DMF, methanol, and ethanol, respectively. Finally, a white precipitate was obtained. The product was dried and dispersed in ethanol as a solution with a concentration of 2 mg / mL. After that, BNQDs were embedded in MOF nanomaterials. Briefly, MOF was carboxyl activated by 20 mM EDC and 10 mM NHS, and then 8 mL of BNQDs aqueous solution (2 mg / mL) was mixed with 10 mL MOF dispersion, and the solution was stirred at 95 °C for 15 h, and then ethanol and ultrapure water were centrifuged. The obtained product was dispersed in water and stored at 4 °C for further work.
[0032] Example 2
[0033] The electroluminescent material of metal organic framework enriched boron nitride quantum dots comprises the following steps during preparation:
[0034] (1) Preparation of Boron Nitride Quantum Dots (BNQDs)
[0035] First, 1.2 g HBO3 was added to 30 ml ultrapure water and ultrasonicated for 5 min to obtain a homogeneous solution. Then 2.4 mL of concentrated ammonia was added and stirred evenly. The obtained solution was transferred to an autoclave and heated to 200 °C for 12 h to obtain a uniform and transparent solution. The pH value was adjusted to 7.0 with 0.1 M HCl. After centrifugation, the obtained product was dispersed in water and stored in a refrigerator at 4 °C for later use.
[0036] (2) Preparation of BNQDs@MOF
[0037] 45 mg of BPDC was dispersed in DMF containing 360 μL of triethylamine as an organic ligand precursor solution. 45 mg of ZrCl4 was ultrasonically dispersed in 16 mL of DMF as a white metal precursor solution. Then, the two solutions were mixed with 2.25 mL of acetic acid, transferred to a Teflon-sealed autoclave for high-pressure reaction, and left to stand at 90 °C for 24 h. After the solvothermal reaction, it was centrifuged at 6500 rpm for 12 min and then washed with DMF, methanol, and ethanol, respectively. Finally, a white precipitate was obtained. The product was dried and dispersed in ethanol as a solution with a concentration of 2 mg / mL. After that, BNQDs were embedded in MOF nanomaterials. Briefly, MOF was carboxyl activated by 20 mM EDC and 10 mM NHS, and then 10 mL of BNQDs solution (2 mg / mL) was mixed with 10 mL of MOF dispersion, and the solution was stirred at 95 °C for 15 h, and then ethanol and ultrapure water were centrifuged. The obtained product was dispersed in water and stored at 4 °C for further work.
[0038] Example 3
[0039] The electroluminescent material of metal organic framework enriched boron nitride quantum dots comprises the following steps during preparation:
[0040] (1) Preparation of Boron Nitride Quantum Dots (BNQDs)
[0041] First, 1.4 g HBO3 was added to 30 ml ultrapure water and ultrasonicated for 5 min to obtain a homogeneous solution. Then 2.4 mL of concentrated ammonia was added and stirred evenly. The obtained solution was transferred to an autoclave and heated to 200 °C for 12 h to obtain a uniform and transparent solution. The pH value was adjusted to 7.0 with 0.1 M HCl. After centrifugation, the obtained product was dispersed in water and stored in a refrigerator at 4 °C for later use.
[0042] (2) Preparation of BNQDs@MOF
[0043] 50 mg BPDC was dispersed in DMF containing 360 μL triethylamine as an organic ligand precursor solution. 45 mg ZrCl4 was ultrasonically dispersed in 16 mL DMF as a white metal precursor solution. Then, the two solutions were mixed with 2.25 mL acetic acid, transferred to a Teflon-sealed autoclave for high-pressure reaction, and left to stand at 90°C for 24 h. After the solvothermal reaction, it was centrifuged at 6500 rpm for 12 min and then washed with DMF, methanol, and ethanol, respectively. Finally, a white precipitate was obtained. The product was dried and dispersed in ethanol as a solution with a concentration of 2 mg / mL. After that, BNQDs were embedded in MOF nanomaterials. Briefly, MOF was carboxyl activated by 20 mM EDC and 10 mM NHS, and then 10 mL BNQDs solution (2 mg / mL) was mixed with 10 mL MOF dispersion, and the solution was stirred at 95°C for 15 h, and then ethanol and ultrapure water were centrifuged. The obtained product was dispersed in water and stored at 4 °C for further work.
[0044] Embodiment 4:
[0045] The BNQDs@MOF material obtained in Example 1 was used to prepare an electroluminescent sensor, and the specific steps were as follows:
[0046] (1) A glassy carbon electrode (GCE) with a diameter of 4 mm was polished into a mirror surface using 1.0, 0.3, and 0.05 µm alumina polishing powders in sequence, and then thoroughly cleaned by ultrasonication in anhydrous ethanol and ultrapure water.
[0047] (2) Then, the GCE was placed in a 0.1 mol / L PBS (pH 7.4) and 3.0 mmol / L (p-aminobenzoic acid) p-ABA solution and scanned for 3 cycles between 0.40 and 1.20 V at a speed of 10 mV / s to fix p-aminobenzoic acid to the electrode surface. The electrode surface was rinsed with ultrapure water and dried at room temperature to obtain GCE|ABA.
[0048] (3) Continue to take 6 μL of the freshly prepared mixed solution containing 20 mg / mL EDC and 10 mg / mL NHS and drop it onto the electrode surface. Incubate at 37°C for 1 h to activate the carboxyl groups of ABA on the electrode surface. Then rinse the electrode surface with pH = 7.38 phosphate buffer and dry it at room temperature.
[0049] (4) Continue to add 6 µL of 5.0 µg / mL trenbolone (TBE) capture antibody onto the electrode surface and dry in a 4°C refrigerator.
[0050] (5) Continue to add 3.0 μL of 0.8 mg / mL bovine serum albumin solution to the electrode surface to block nonspecific active sites on the electrode surface, rinse the electrode surface with pH = 7.38 phosphate buffer, and dry in a 4°C refrigerator;
[0051] (6) Add 6.0 µL of a series of different concentrations of trenbolone (TBE) antigen solutions ranging from 0.0001 to 40 ng / mL, rinse the electrode surface with pH = 7.38 phosphate buffer, and dry in a refrigerator at 4°C.
[0052] (7) The BNQDs@MOF prepared in Example 1 and the detection antibody (100 µL, 8 µM) were gently shaken at room temperature for 5 h. Then, the free antibody was removed by centrifugation and the complex was redispersed in a buffer solution. Finally, a BNQDs@MOF-labeled trenbolone detection antibody solution was obtained and stored at 4°C until use.
[0053] (8) Finally, 6 μL of 1.0 mg / mL BNQDs@MOF-labeled trenbolone (TBE) detection antibody solution was dropped onto the electrode and incubated at room temperature for 1 hour. The solution was then washed with ultrapure water to obtain an electrochemiluminescent sensor based on metal organic framework-accelerated enrichment of boron nitride quantum dots. The sensor was then stored in a refrigerator at 4°C for future use.
[0054] Example 5
[0055] A method for preparing an electrochemiluminescent sensor based on metal organic framework accelerated enrichment of boron nitride quantum dots for luminescence comprises the following steps:
[0056] (1) A glassy carbon electrode with a diameter of 4 mm was polished into a mirror surface using 1.0, 0.3 and 0.05 µm alumina polishing powders in sequence, and then thoroughly cleaned by ultrasonication in anhydrous ethanol and ultrapure water.
[0057] (2) Then, p-aminobenzoic acid was fixed to the electrode surface by placing GCE in 0.1 mol / L PBS (pH 7.4) and 5.0 mmol / L p-ABA solution and scanning at a speed of 0.1 V / s between 0.40 and 1.20 V for 3 cycles. The electrode surface was rinsed with ultrapure water and dried at room temperature to obtain GCE|ABA.
[0058] (3) Continue to take 6 μL of a freshly prepared mixed solution containing 20 mg / mL EDC and 10 mg / mL NHS and add it to the electrode surface. Incubate at 37°C for 1 h to activate the carboxyl groups of ABA on the electrode surface. Then rinse the electrode surface with pH = 7.38 phosphate buffer and dry it at room temperature.
[0059] (4) Continue to add 6 µL of 10.0 µg / mL trenbolone (TBE) capture antibody onto the electrode surface and dry in a 4°C refrigerator.
[0060] (5) Continue to add 3.0 μL of 1.0 mg / mL bovine serum albumin solution to the electrode surface to block the nonspecific active sites on the electrode surface. Rinse the electrode surface with pH = 7.38 phosphate buffer and dry it in a 4°C refrigerator.
[0061] (6) Add 6.0 µL of a series of different concentrations of trenbolone (TBE) antigen solution ranging from 0.0001 to 40 ng / mL, rinse the electrode surface with pH = 7.38 phosphate buffer, and dry in a refrigerator at 4°C.
[0062] (7) The BNQDs@MOF (2 mg / mL) prepared in Example 2 and the detection antibody (100 µL, 10 µM) were gently shaken at room temperature for 5 hours. Then, the free antibody was removed by centrifugation and washing, and the complex was redispersed in the buffer. Finally, the BNQDs@MOF-labeled trenbolone detection antibody solution was obtained and stored at 4°C until use.
[0063] (8) Finally, 6 μL of 2.0 mg / mL BNQDs@MOF-labeled trenbolone (TBE) detection antibody solution was dropped onto the electrode and incubated at room temperature for 1 hour. The solution was then washed with ultrapure water to obtain an electrochemiluminescent sensor based on metal organic framework-accelerated enrichment of boron nitride quantum dots. The sensor was then stored in a refrigerator at 4°C for future use.
[0064] Example 6
[0065] A method for preparing an electrochemiluminescent sensor based on metal organic framework accelerated enrichment of boron nitride quantum dots for luminescence comprises the following steps:
[0066] (1) A glassy carbon electrode with a diameter of 4 mm was polished into a mirror surface using 1.0, 0.3 and 0.05 µm alumina polishing powders in sequence, and then thoroughly cleaned by ultrasonication in anhydrous ethanol and ultrapure water;
[0067] (2) Then, p-aminobenzoic acid was fixed to the electrode surface by placing GCE in 0.1 mol / L PBS (pH 7.4) and 7.0 mmol / L p-ABA solution and scanning at a speed of 10 mV / s between 0.40 and 1.20 V for 3 cycles. The electrode surface was rinsed with ultrapure water and dried at room temperature to obtain GCE|ABA.
[0068] (3) Continue to take 6 μL of the freshly prepared mixed solution containing 20 mg / mL EDC and 10 mg / mL NHS and drop it onto the electrode surface. Incubate at 37°C for 1 h to activate the carboxyl groups of ABA on the electrode surface. Then rinse the electrode surface with pH = 7.38 phosphate buffer and dry it at room temperature.
[0069] (4) Continue to add 6 µL, 15.0 µg / mL trenbolone (TBE) capture antibody to the electrode surface and dry in a 4°C refrigerator;
[0070] (5) Continue to add 3.0 μL of 1.2 mg / mL bovine serum albumin solution to the electrode surface to block nonspecific active sites on the electrode surface, rinse the electrode surface with pH = 7.38 phosphate buffer, and dry in a 4°C refrigerator;
[0071] (6) Add 6.0 µL of a series of different concentrations of trenbolone (TBE) antigen solutions ranging from 0.0001 to 40 ng / mL, rinse the electrode surface with pH = 7.38 phosphate buffer, and dry in a refrigerator at 4°C;
[0072] (7) The prepared BNQDs@MOF (2 mg / mL) and the detection antibody (100 µL, 10 µM) obtained in Example 3 were gently shaken at room temperature for 5 hours. Then, the free antibody was removed by centrifugation and the complex was redispersed in the buffer. Finally, the BNQDs@MOF-labeled trenbolone detection antibody solution was obtained and stored at 4°C until use.
[0073] (8) Finally, 6 μL of 3.0 mg / mL BNQDs@MOF-labeled trenbolone (TBE) detection antibody solution was dropped onto the electrode and incubated at room temperature for 1 hour. The solution was then washed with ultrapure water to obtain an electrochemiluminescent sensor based on metal organic framework-accelerated enrichment of boron nitride quantum dots. The sensor was then stored in a refrigerator at 4°C for future use.
[0074] Example 7
[0075] The sensor prepared in Example 4 was used to detect trenbolone in environmental water, and the steps were as follows:
[0076] (1) The electrochemical workstation was used for testing with a three-electrode system. The Ag / AgCl electrode was used as the reference electrode, the platinum wire electrode was used as the auxiliary electrode, and the prepared electrochemiluminescence sensor based on the luminescence of metal organic framework-enriched boron nitride quantum dots was used as the working electrode. The high voltage of the photomultiplier tube was set to 500 V, the scanning potential was 0~-2.0 V, and the scanning rate was 0.1 V / s.
[0077] (2) In 10 mL of phosphate buffer solution containing 100 mmol / L potassium persulfate at pH 7.4, the electrochemiluminescence signal intensity generated by different concentrations of the analyte antigen was detected by an electrochemiluminescence system, and a working curve was drawn;
[0078] (3) The sample solution to be tested is used instead of the trenbolone antigen solution for testing.
[0079] The above embodiments are only for illustrating the technical ideas and features of the present invention, and the contents are only preferred embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Within the technical scope disclosed by the present invention, equivalent changes or improvements made according to the technical solution and inventive concept of the present invention should be included in the protection scope of the present invention.
Claims
1. Use of an electrochemiluminescent sensor prepared from an electroluminescent material in the detection of trenbolone (TBE), characterized in that: The preparation of the electrochemiluminescent sensor prepared by the electroluminescent material comprises the following steps: S1. Polish the glassy carbon electrode with alumina and clean it; then place it in p-aminobenzoic acid buffer for electropolymerization, clean and dry it; then use a mixed solution of EDC and NHS to drip onto the electrode surface for treatment, and finally clean and dry it; S2, dripping the trenbolone capture antibody to be detected onto the electrode surface obtained in S1, drying, then dripping bovine serum albumin solution onto the electrode surface to block the non-specific active sites on the electrode surface, washing and drying; dripping a series of trenbolone antigen solutions of different concentrations to be detected onto the electrode surface, washing and drying again; S3, preparing BNQDs@MOF into a dispersion, adding the detection antibody of the analyte to be tested and mixing at room temperature for 4-6 hours, centrifuging and dispersing into a buffer to prepare a BNQDs@MOF-labeled analyte trenbolone detection antibody solution; S4, dropping the BNQDs@MOF-labeled trenbolone detection antibody solution obtained in S3 onto the electrode obtained in S2, incubating at room temperature and then washing to prepare an electrochemiluminescent sensor based on metal organic framework-enriched boron nitride quantum dots; Among them, BNQDs@MOF is an electroluminescent material enriched with boron nitride quantum dots in a metal organic framework, and the metal organic framework is specifically a Zr-MOF nanomaterial, and the mass ratio of the Zr-MOF nanomaterial to the boron nitride quantum dots BNQDs is 1:0.8~1.2; When preparing BNQDs@MOF, Zr-MOF nanomaterials were dispersed with ethanol, carboxyl groups were activated by 20 mM EDC and 10 mM NHS, and boron nitride quantum dots were dispersed with water. The two were then mixed in proportion, and the solution was stirred at 90-100 °C for 12-18 hours. After centrifugation, the solution was washed with ethanol and ultrapure water respectively to obtain BNQDs@MOF. When preparing Zr-MOF nanomaterials, 4,4'-biphenyldicarboxylic acid (BPDC) is used as an organic ligand precursor and ZrCl4 is used as a metal precursor. The two are dispersed in a solution and mixed, and acetic acid is added and heated to react. After the reaction, the reaction is centrifuged, washed and dried to obtain the material. When preparing boron nitride quantum dots, HBO3 and ammonia water are used as raw materials. After heating and reaction, the pH is adjusted to neutral and centrifuged to obtain the material.
2. The use according to claim 1, characterized in that: The glassy carbon electrode in S1 was polished with aluminum oxide particles from coarse to fine in sequence until the surface was mirror-like, and then cleaned with anhydrous ethanol and ultrapure water in sequence.
3. The use according to claim 1, characterized in that: The p-aminobenzoic acid buffer in S1 is a mixture of 3.0~7.0mmol / L p-aminobenzoic acid solution and PBS buffer solution. During treatment, the electrode is placed in the mixed solution and scanned at 0.40~1.20V for 3 cycles at a speed of 10mV / s to fix p-aminobenzoic acid to the electrode surface, rinsed with ultrapure water, and dried at room temperature. When treating with EDC and NHS, a mixed solution of 20 mg / mL EDC and 10 mg / mL NHS is added dropwise to the electrode surface, incubated at 35~38℃ for 1~1.5h, rinsed the electrode surface with phosphate buffer, and dried at room temperature.
4. The use according to claim 1, characterized in that: The concentration of the capture antibody of the analyte in S2 is 5.0~15.0µg / mL; the concentration of the bovine serum albumin solution is 0.8~1.2mg / mL; a series of different concentrations of the analyte antigen solution are between 0.0001~40ng / mL; phosphate buffer is used for washing in S2, and it is dried in a refrigerator at 4°C.
5. The use according to claim 1, characterized in that: In S3, BNQDs@MOF was dispersed in DMF at a concentration of 2 mg / mL, and the concentration of the analyte detection antibody was 8–12 µM; The concentration of the analyte detection antibody solution labeled with BNQDs@MOF in S4 was 1.0~3.0 mg / mL.
Citation Information
Patent Citations
Spectral electrochemiluminescent immunodetection method based on CdZnSe three-component quantum dots
CN106053823A
Preparation method for ultrathin boron nitride nanosheets and dispersion liquid thereof
CN108529574A
Method for preparing electrochemical luminescence sensor for detecting N-terminal brain natriuretic peptide precursor by quantum dot functionalized metal organic frame structure
CN110456071A
UiO@Pd@UiO catalyst, preparation method and applications thereof
CN110947428A
Boron nitride quantum dot / porous metal organic framework composite photocatalytic material as well as preparation method and application thereof
CN112844484A