Injection mold with high hardness and wear-resistant coating and preparation method thereof
By using a specific ratio of coatings and processes, modified graphene and polyphenylene sulfide form a high-hardness wear-resistant coating, which solves the adhesion problem between the mold and the polymer and improves the surface performance and processing of the injection mold. stability.
Patent Information
- Application Number
- CN202311248586.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-26
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-09-26
AI Technical Summary
During the molding and injection molding process of polymers, the adhesion problem between the metal mold and the polymer results in poor apparent quality and size of the injection molded products. The existing coating materials have insufficient hardness and wear resistance, which increases the Processing complexity.
A coating using 65 to 85 parts of polytetrafluoroethylene, 15 to 20 parts of polyphenylene sulfide, 9.1 to 15.0 parts of filler, 1.4 to 2.0 parts of additives, and 260 to 338 parts of solvent is sprayed, dried and The coating is formed through the sintering process, and graphene is modified with components such as polyvinylpyrrolidone and ethyl orthosilicate to increase the hardness and wear resistance of the coating, and polyphenylene sulfide is modified with p-chloroaniline to improve adhesion and Cross-link density.
It significantly improves the hardness, wear resistance and anti-adhesion properties of the injection mold coating, reduces the friction coefficient and wear rate, enhances the adhesion between the coating and the metal mold, and simplifies the processing process.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of mold coatings, in particular to an injection mold with a high-hardness wear-resistant coating and a preparation method thereof. Background Art
[0002] The use of metal molds is indispensable in the molding and injection molding of high molecular polymers. In the mold and injection molding industry, polymers have strong adsorption and carry active groups, which are easy to adhere to metal molds, which will have a negative impact on the apparent quality and size of the injection molded products, greatly increasing the complexity of processing. A coating needs to be provided on the surface of the mold to separate the injection molded plastic from the metal mold, among which polytetrafluoroethylene is a commonly used coating material. However, there is still room for improvement in its hardness and wear resistance. Therefore, we propose an injection mold with a high hardness and wear-resistant coating and a preparation method thereof. Summary of the invention
[0003] The object of the present invention is to provide an injection mold with a high-hardness wear-resistant coating and a preparation method thereof, so as to solve the problems raised in the above background technology.
[0004] In order to solve the above technical problems, the present invention provides the following technical solutions: a method for preparing an injection mold with a high-hardness wear-resistant coating, comprising the following processes:
[0005] The coating is sprayed on the mold surface, dried, and sintered to form a coating to obtain an injection mold.
[0006] Further, the coating comprises the following components by mass: 65 to 85 parts of polytetrafluoroethylene, 15 to 20 parts of polyphenylene sulfide, 9.1 to 15.0 parts of filler, 1.4 to 2.0 parts of additive, and 260 to 338 parts of solvent;
[0007] The filler comprises 8 to 12 parts of graphene and 1.1 to 3.0 parts of molybdenum disulfide.
[0008] Further, the solvent includes 104 to 134 parts by mass of ethanol, 26 to 34 parts by mass of dimethylacetamide and 130 to 170 parts by mass of deionized water;
[0009] The auxiliary agent comprises 0.1 to 0.2 parts by weight of a leveling agent, 0.3 to 0.5 parts by weight of a defoaming agent, 0.3 to 0.5 parts by weight of a surfactant and 0.7 to 0.8 parts by weight of a film-forming auxiliary agent.
[0010] Leveling agent: TEGO Glide 410, from Foshan Sansheng Trading Co., Ltd.; defoamer: TSA-4701, from Jiangsu Tengda Additive Co., Ltd.; surfactant is sodium dodecylbenzene sulfonate; film-forming aid is ester alcohol dodecahydrate;
[0011] Polytetrafluoroethylene: powder, particle size 1250 mesh, from DuPont, USA;
[0012] Polyphenylene sulfide (PPS): PR06, from Chevron Phillips, USA;
[0013] Molybdenum disulfide: particle size 2000 mesh, sourced from Henan Xinding Chemical Co., Ltd.;
[0014] Graphene: Single-layer graphene, particle size 300-500nm, sourced from Suzhou Carbonfeng Graphene Technology Co., Ltd.
[0015] Furthermore, the polyphenylene sulfide is grafted and modified, and the specific process is as follows:
[0016] Take polyphenylene sulfide, p-chloroaniline, sodium hydroxide and 1-methyl-pyrrolidone and mix them. Under the protection of nitrogen atmosphere, heat them to 245-255° C. and keep them warm for 180-220 min. Cool them to 215-225° C. and keep them warm for 18-24 min. Cool them to 120-140° C., filter and wash them to obtain amino-terminated polyphenylene sulfide.
[0017] Take amino-terminated polyphenylene sulfide, aniline, 2-fluoroaniline, ammonium persulfate and sulfuric acid solution, mix them at 0-2°C, put them in an autoclave, react for 4-7 hours at a temperature of 3-5°C and a pressure of 0.1-1.0 MPa; filter and wash to obtain modified polyphenylene sulfide.
[0018] Further, the ratio of polyphenylene sulfide, p-chloroaniline, sodium hydroxide, and 1-methyl-pyrrolidone is 24 g: (0.5-0.6) g: (0.7-0.8) g: 100 mL;
[0019] The ratio of amino-terminated polyphenylene sulfide, aniline, 2-fluoroaniline, ammonium persulfate, and sulfuric acid solution is 20 g: (0.25-0.46) g: (0.28-0.55) g: (1.3-2.4) g: 100 mL;
[0020] The concentration of the sulfuric acid solution was 1M.
[0021] Further, the graphene of some component qualities is compounded, and the specific process is as follows:
[0022] The graphene is dispersed in deionized water, polyvinyl pyrrolidone is added, ethanol and sodium citrate dihydrate are added in sequence and mixed evenly, ammonia water and ethyl orthosilicate are added, the temperature is raised to 88-94° C. and the mixture is reacted for 120-180 minutes; the mixture is filtered and washed to obtain composite graphene.
[0023] Further, the ratio of graphene, deionized water, ethanol, and ammonia water is 10 g: 100 mL: 28-30 mL: 10 mL;
[0024] The mass ratio of graphene, polyvinyl pyrrolidone, sodium citrate dihydrate, and tetraethyl orthosilicate is 5:(5.6-11.3):(0.04-0.08):(0.5-1.0);
[0025] Polyvinyl pyrrolidone was added in the form of n-pentanol solution with a mass concentration of 10%;
[0026] Sodium citrate dihydrate was added as an aqueous solution at a concentration of 0.18 M;
[0027] Polyvinylpyrrolidone (PVP): average molecular weight 58,000, sourced from Guangzhou Yuemei Chemical Co., Ltd.
[0028] Furthermore, the filler includes the following components by mass: 5 to 6 parts of graphene, 3 to 6 parts of composite graphene, and 1.1 to 3.0 parts of molybdenum disulfide.
[0029] Furthermore, the filler is modified by coupling with KH560, and the specific process is as follows:
[0030] Mix KH560 and ethanol solution, heat to 60-70°C and stir for 7-12 minutes, add filler, and continue stirring for 60-90 minutes; cool, centrifuge, and wash to obtain modified filler;
[0031] The ratio of KH560, filler, and ethanol solution is (0.7-1.0) g:20 g:100 mL;
[0032] The mass fraction of the ethanol solution is 95%.
[0033] Furthermore, the process conditions of the spraying are: spraying pressure 0.2-0.3 MPa, nozzle diameter 1.8 mm, distance between the nozzle and the mold 200-250 mm, and spraying rate 6-8 m / min.
[0034] Furthermore, the drying process conditions are: temperature 80-95° C., time 4-10 min.
[0035] Furthermore, the sintering process conditions are: 280-290° C., baking and heat preservation for 75-100 minutes, removal of additives and low molecular weight polymers, etc.; 360-380° C., curing and heat preservation for 12-18 minutes, and cooling with the furnace.
[0036] Furthermore, the spraying thickness is 20-40 μm.
[0037] Furthermore, the mold base is subjected to surface treatment before processing, and the processes are cleaning and sandblasting in sequence;
[0038] The cleaning process is: alkali washing, water washing, acid washing, alkali neutralization, water washing;
[0039] Alkaline washing process: 1M sodium hydroxide solution for 10-15 minutes, the temperature of the sodium hydroxide solution is 40-60°C;
[0040] The pickling process is: immersion in 8-10wt% hydrochloric acid for 5 minutes, the hydrochloric acid temperature is 55-62°C;
[0041] The alkali neutralization process is carried out in 8-10 wt% sodium hydroxide solution, and the solution is taken out after no more floccules are precipitated.
[0042] Furthermore, the sandblasting process is as follows: sandblasting distance 15 cm, spray angle 45° to 75°, sandblasting time 5 min, compressed air 0.5 to 0.6 MPa;
[0043] Furthermore, the mold is made of hard aluminum, 45# steel or 304 stainless steel.
[0044] In the above technical scheme, components such as polyvinyl pyrrolidone and tetraethyl orthosilicate deposit linear silica on the surface of part of the graphene, so that multi-branched structural protrusions appear on the surface of its two-dimensional structure, and linear silica-compounded graphene is obtained, which is recorded as composite graphene. It is compounded with uncompounded graphene and molybdenum disulfide to promote the adsorption between the coating and the metal mold; and in the drying and sintering stages, small molecular components such as additives and solvents float and detach, and promote the selective orientation and arrangement of the filler, promote the flat coverage of fillers such as flaky graphene, reduce the thickness of the coating, and reduce the spacing between the coating components, so that the composite structure of the composite graphene is connected with the graphene, and its diameter avoids the overlap between layered graphene and molybdenum disulfide, and can give full play to the rigidity and lubricity of the filler graphene and molybdenum disulfide, and improve the hardness and anti-sticking, wear resistance and impact resistance of the prepared coating. Finally, the filler was coupled and modified, KH570 was used to improve the dispersion of the filler in the resin matrix, and epoxy groups were introduced to facilitate the reaction in the subsequent process.
[0045] Polyphenylene sulfide is a thermoplastic resin containing phenylthio groups in the main chain of the molecule. It has strong rigidity and regularity, high strength and modulus, and stable dimensions. After mixing with polytetrafluoroethylene, it can improve the wear resistance of the prepared coating, and can improve the adhesion between the coating and the mold, and promote the improvement of its comprehensive performance. The end groups of polyphenylene sulfide are modified by parachloroaniline, wherein the chlorine group in parachloroaniline reacts with the thiol group in polyphenylene sulfide to convert the end groups into aniline groups; then, under high pressure, it is copolymerized with aniline and 2-fluoroaniline to obtain polyphenylene sulfide modified with fluoropolyaniline, which is recorded as modified polyphenylene sulfide, which can improve the adhesion of the coating on the surface of the metal mold; in the drying and sintering process, it reacts with the epoxy groups in the modified filler to solidify, increase the crosslinking density of the coating, and improve its wear resistance; and the introduction of fluorine atoms with low surface energy and extremely small radius can reduce the friction coefficient and abrasive of the coating, and further improve the wear resistance and anti-sticking ability of the coating.
[0046] Compared with the prior art, the present invention has the following beneficial effects:
[0047] 1. The injection mold with high hardness and wear-resistant coating and the preparation method thereof of the present invention deposit linear silicon dioxide on the surface of part of graphene by components such as polyvinyl pyrrolidone and tetraethyl orthosilicate, so that multi-branched structure protrusions appear on the surface of the two-dimensional structure to obtain composite graphene, which is compounded with graphene and molybdenum disulfide to avoid the overlap of layered graphene and molybdenum disulfide, give full play to the rigidity and lubricity of filler graphene and molybdenum disulfide, and improve the hardness and anti-sticking, wear resistance and impact resistance of the prepared coating.
[0048] 2. The injection mold with high hardness and wear-resistant coating and the preparation method thereof of the present invention modify polyphenylene sulfide by using p-chloroaniline to convert the terminal group into an amino group; copolymerize with aniline and 2-fluoroaniline to obtain modified polyphenylene sulfide, and react with the epoxy groups in the modified filler during the drying and sintering process to increase the crosslinking density of the coating and improve its wear resistance; and introduce fluorine atoms with low surface energy and extremely small radius to reduce the friction coefficient and abrasive material of the coating, thereby further improving the wear resistance and anti-sticking ability of the coating. DETAILED DESCRIPTION
[0049] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0050] In the following specific implementations, the group allocation ratio can be expanded in equal proportion.
[0051] Leveling agent: TEGO Glide 410, from Foshan Sansheng Trading Co., Ltd.; defoamer: TSA-4701, from Jiangsu Tengda Additive Co., Ltd.; surfactant is sodium dodecylbenzene sulfonate; film-forming aid is ester alcohol dodecahydrate;
[0052] Polytetrafluoroethylene: powder, particle size 1250 mesh, from DuPont, USA;
[0053] Polyphenylene sulfide (PPS): PR06, from Chevron Phillips, USA;
[0054] Molybdenum disulfide: particle size 2000 mesh, sourced from Henan Xinding Chemical Co., Ltd.;
[0055] Graphene: Single-layer graphene, particle size 300-500nm, sourced from Suzhou Tanfeng Graphene Technology Co., Ltd.;
[0056] Polyvinylpyrrolidone (PVP): average molecular weight 58,000, from Guangzhou Yuemei Chemical Co., Ltd.;
[0057] The mold is made of 45# steel.
[0058] Embodiment 1: A method for preparing an injection mold having a high-hardness wear-resistant coating, comprising the following process:
[0059] Step 1:
[0060] 1.1 Take 24g polyphenylene sulfide, 0.5g p-chloroaniline, 0.7g sodium hydroxide, and 100mL 1-methyl-pyrrolidone and mix them. Under the protection of nitrogen atmosphere, heat them to 245℃ and keep them warm for 220min; cool them to 215℃ and keep them warm for 24min; cool them to 120℃; filter and wash them to obtain amino-terminated polyphenylene sulfide;
[0061] 20 g of amino-terminated polyphenylene sulfide was mixed with 0.25 g of aniline, 0.28 g of 2-fluoroaniline, 1.3 g of ammonium persulfate, and 100 mL of 1 M sulfuric acid solution at 2° C., placed in an autoclave, and reacted for 7 h at a temperature of 3° C. and a pressure of 0.1 MPa; filtered and washed to obtain modified polyphenylene sulfide;
[0062] 1.2 Disperse 10g of graphene in 100mL of deionized water, add polyvinyl pyrrolidone, add 28mL of ethanol and sodium citrate dihydrate in sequence and mix well, add 10mL of ammonia water and ethyl orthosilicate, heat to 88℃ and react for 180min; filter and wash to obtain composite graphene;
[0063] The mass ratio of graphene, polyvinyl pyrrolidone, sodium citrate dihydrate, and tetraethyl orthosilicate is 5:5.6:0.04:0.5; polyvinyl pyrrolidone is added in the form of n-pentanol solution with a mass concentration of 10%; sodium citrate dihydrate is added in the form of aqueous solution with a concentration of 0.18M;
[0064] 1.3 The filler includes the following mass components: 5 parts of graphene, 3 parts of composite graphene, and 1.1 parts of molybdenum disulfide; KH560 and 95% ethanol solution are mixed, heated to 60°C and stirred for 12 minutes, the filler is added, and stirring is continued for 90 minutes; cooled, centrifuged, and washed to obtain a modified filler; the ratio of KH560, filler, and ethanol solution is 0.7g:20g:100mL;
[0065] Step 2, the coating includes the following components by mass: 85 parts of polytetrafluoroethylene, 15 parts of polyphenylene sulfide, 9.1 parts of filler, 1.4 parts of additives, and 338 parts of solvent; the solvent includes 134 parts by mass of ethanol, 34 parts by mass of dimethylacetamide and 170 parts by mass of deionized water; the additives include 0.1 parts by mass of leveling agent, 0.3 parts by mass of defoaming agent, 0.3 parts by mass of surfactant and 0.7 parts by mass of film-forming aid;
[0066] According to the above formula, the components are mixed and stirred at 50°C for 30 minutes to obtain a coating, wherein the defoaming agent in the auxiliary agent is added after stirring; the coating is sprayed on the mold surface, and the spraying process conditions are: spraying pressure 0.2MPa, nozzle diameter 1.8mm, the distance between the nozzle and the mold is 200mm, the spraying rate 6m / min, and the spraying thickness is 40μm; drying, the drying process conditions are: temperature 80°C, time 10min; sintering, the sintering process conditions are: 280°C, baking and heat preservation 100min, 360°C, curing and heat preservation 18min, and cooling with the furnace; forming a coating to obtain an injection mold.
[0067] Embodiment 2: A method for preparing an injection mold having a high-hardness wear-resistant coating, comprising the following process:
[0068] Step 1:
[0069] 1.1 Take 24g polyphenylene sulfide, 0.55g p-chloroaniline, 0.75g sodium hydroxide, and 100mL 1-methyl-pyrrolidone and mix them. Under the protection of nitrogen atmosphere, heat them to 250℃ and keep them warm for 200min; cool them to 220℃ and keep them warm for 21min; cool them to 130℃; filter and wash them to obtain amino-terminated polyphenylene sulfide;
[0070] 20 g of amino-terminated polyphenylene sulfide was mixed with 0.35 g of aniline, 0.41 g of 2-fluoroaniline, 1.8 g of ammonium persulfate, and 100 mL of 1 M sulfuric acid solution at 1°C, placed in an autoclave, and reacted for 5 h at 4°C and 0.5 MPa; filtered and washed to obtain modified polyphenylene sulfide;
[0071] 1.2 Disperse 10g of graphene in 100mL of deionized water, add polyvinyl pyrrolidone, add 29mL of ethanol and sodium citrate dihydrate in sequence and mix well, add 10mL of ammonia water and ethyl orthosilicate, heat to 90℃ and react for 150min; filter and wash to obtain composite graphene;
[0072] The mass ratio of graphene, polyvinyl pyrrolidone, sodium citrate dihydrate, and tetraethyl orthosilicate is 5:8.5:0.06:0.8; polyvinyl pyrrolidone is added in the form of n-pentanol solution with a mass concentration of 10%; sodium citrate dihydrate is added in the form of aqueous solution with a concentration of 0.18M;
[0073] 1.3 The filler includes the following mass components: 5.5 parts of graphene, 4.5 parts of composite graphene, and 2.0 parts of molybdenum disulfide; KH560 and 95% ethanol solution are mixed, heated to 65°C and stirred for 10 minutes, the filler is added, and stirring is continued for 75 minutes; cooling, centrifugation, and washing are performed to obtain a modified filler; the ratio of KH560, filler, and ethanol solution is 0.8g:20g:100mL;
[0074] Step 2, the coating includes the following components by mass: 75 parts of polytetrafluoroethylene, 18 parts of polyphenylene sulfide, 12.0 parts of filler, 1.7 parts of additives, and 300 parts of solvent; the solvent includes 120 parts by mass of ethanol, 30 parts by mass of dimethylacetamide and 150 parts by mass of deionized water; the additives include 0.15 parts by mass of leveling agent, 0.4 parts by mass of defoamer, 0.4 parts by mass of surfactant and 0.75 parts by mass of film-forming aid;
[0075] According to the above formula, the components are mixed at 50°C and stirred for 30 minutes to obtain a coating, wherein the defoamer in the auxiliary agent is added after stirring; the coating is sprayed on the mold surface, and the spraying process conditions are: spraying pressure 0.25MPa, nozzle diameter 1.8mm, distance between the nozzle and the mold is 225mm, spraying rate 7m / min, and spraying thickness 40μm; drying, the drying process conditions are: temperature 88°C, time 7min; sintering, the sintering process conditions are: 285°C, baking and heat preservation 90min, 370°C, curing and heat preservation 15min, and cooling with the furnace; forming a coating to obtain an injection mold
[0076] Embodiment 3: A method for preparing an injection mold having a high-hardness wear-resistant coating, comprising the following process:
[0077] Step 1:
[0078] 1.1 Take 24g polyphenylene sulfide, 0.6g p-chloroaniline, 0.8g sodium hydroxide, and 100mL 1-methyl-pyrrolidone and mix them. Under the protection of nitrogen atmosphere, heat them to 255℃ and keep them warm for 180min; cool them to 225℃ and keep them warm for 18min; cool them to 140℃; filter and wash them to obtain amino-terminated polyphenylene sulfide;
[0079] 20 g of amino-terminated polyphenylene sulfide was mixed with 0.46 g of aniline, 0.55 g of 2-fluoroaniline, 2.4 g of ammonium persulfate, and 100 mL of 1 M sulfuric acid solution at 0° C., placed in an autoclave, and reacted for 4 h at a temperature of 5° C. and a pressure of 1.0 MPa; filtered and washed to obtain modified polyphenylene sulfide;
[0080] 1.2 Disperse 10g of graphene in 100mL of deionized water, add polyvinyl pyrrolidone, add 30mL of ethanol and sodium citrate dihydrate in sequence and mix well, add 10mL of ammonia water and ethyl orthosilicate, heat to 94℃ and react for 120min; filter and wash to obtain composite graphene;
[0081] The mass ratio of graphene, polyvinyl pyrrolidone, sodium citrate dihydrate, and tetraethyl orthosilicate is 5:11.3:0.08:1.0; polyvinyl pyrrolidone is added in the form of n-pentanol solution with a mass concentration of 10%; sodium citrate dihydrate is added in the form of aqueous solution with a concentration of 0.18M;
[0082] 1.3 The filler includes the following mass components: 6 parts of graphene, 6 parts of composite graphene, and 3.0 parts of molybdenum disulfide; KH560 and 95% ethanol solution are mixed, heated to 70°C and stirred for 7 minutes, the filler is added, and stirring is continued for 60 minutes; cooling, centrifugation, and washing are performed to obtain a modified filler; the ratio of KH560, filler, and ethanol solution is 1.0g:20g:100mL;
[0083] Step 2, the coating includes the following components by mass: 65 parts of polytetrafluoroethylene, 20 parts of polyphenylene sulfide, 15.0 parts of filler, 2.0 parts of additives, and 260 parts of solvent; the solvent includes 104 parts by mass of ethanol, 26 parts by mass of dimethylacetamide and 130 parts by mass of deionized water; the additives include 0.2 parts by mass of leveling agent, 0.5 parts by mass of defoamer, 0.5 parts by mass of surfactant and 0.8 parts by mass of film-forming aid;
[0084] According to the above formula, the components are mixed and stirred at 50°C for 30 minutes to obtain a coating, wherein the defoaming agent in the auxiliary agent is added after stirring; the coating is sprayed on the mold surface, and the spraying process conditions are: spraying pressure 0.3MPa, nozzle diameter 1.8mm, the distance between the nozzle and the mold is 250mm, the spraying rate 8m / min, and the spraying thickness is 40μm; drying, the drying process conditions are: temperature 95°C, time 4min; sintering, the sintering process conditions are: 290°C, baking and heat preservation 75min, 380°C, curing and heat preservation 12min, and cooling with the furnace; forming a coating to obtain an injection mold.
[0085] Comparative Example 1: A method for preparing an injection mold having a high hardness and wear-resistant coating,
[0086] Step 1:
[0087] 1.1 Take 24g polyphenylene sulfide, 0.5g p-chloroaniline, 0.7g sodium hydroxide, and 100mL 1-methyl-pyrrolidone and mix them. Under the protection of nitrogen atmosphere, heat them to 245℃ and keep them warm for 220min; cool them to 215℃ and keep them warm for 24min; cool them to 120℃; filter and wash them to obtain amino-terminated polyphenylene sulfide;
[0088] 20 g of amino-terminated polyphenylene sulfide was mixed with 0.25 g of aniline, 0.28 g of 2-fluoroaniline, 1.3 g of ammonium persulfate, and 100 mL of 1 M sulfuric acid solution at 2° C., placed in an autoclave, and reacted for 7 h at a temperature of 3° C. and a pressure of 0.1 MPa; filtered and washed to obtain modified polyphenylene sulfide;
[0089] 1.2 The filler includes the following mass components: 8 parts of graphene and 1.1 parts of molybdenum disulfide; KH560 and 95% ethanol solution are mixed, heated to 60°C and stirred for 12 minutes, the filler is added, and stirring is continued for 90 minutes; cooled, centrifuged, and washed to obtain a modified filler; the ratio of KH560, filler, and ethanol solution is 0.7g:20g:100mL;
[0090] Step 2 is the same as in Example 1, obtaining an injection mold.
[0091] Comparative Example 2: A method for preparing an injection mold having a high hardness and wear-resistant coating,
[0092] Step 1:
[0093] 1.1 Take 24g polyphenylene sulfide, 0.5g p-chloroaniline, 0.7g sodium hydroxide, and 100mL 1-methyl-pyrrolidone, mix them, and under the protection of nitrogen atmosphere, heat them to 245℃, keep them warm for 220min; cool them to 215℃, keep them warm for 24min; cool them to 120℃; filter and wash them to obtain modified polyphenylene sulfide;
[0094] 1.2 The filler includes the following mass components: 8 parts of graphene and 1.1 parts of molybdenum disulfide; KH560 and 95% ethanol solution are mixed, heated to 60°C and stirred for 12 minutes, the filler is added, and stirring is continued for 90 minutes; cooled, centrifuged, and washed to obtain a modified filler; the ratio of KH560, filler, and ethanol solution is 0.7g:20g:100mL;
[0095] Step 2 is the same as in Example 1, obtaining an injection mold.
[0096] Comparative Example 3: A method for preparing an injection mold having a high hardness and wear-resistant coating,
[0097] Step 1: The filler includes the following mass components: 9.1 parts of graphene; KH560 and 95% ethanol solution are mixed, heated to 60°C and stirred for 12 minutes, the filler is added, and stirring is continued for 90 minutes; cooling, centrifugation, and washing to obtain a modified filler; the ratio of KH560, filler, and ethanol solution is 0.7g:20g:100mL;
[0098] Step 2, replacing the modified polyphenylene sulfide with polyphenylene sulfide of equal mass, and other processes are the same as those in Example 1 to obtain an injection mold.
[0099] Experiment: Take the injection molds obtained in Examples 1-3 and Comparative Examples 1-3, make samples, test their properties respectively and record the test results:
[0100] Hardness test: Using GB / T5739 as reference standard, test the pencil hardness of the coating;
[0101] Adhesion test: GB / T9286 is used as the reference standard to test the adhesion level of the coating;
[0102] Anti-stick performance test: A contact angle meter was used to test the contact angle of the coating as an indicator of anti-stick performance. Deionized water was used in the test, and the water droplet volume was 5 μL.
[0103] Wear resistance test: A ball-disc friction and wear testing machine was used to test the friction coefficient of the coating. The counterpart was a GCr15 steel ball with a diameter of 3.175 mm, the center diameter of the wear track was 12 mm, the experimental load was 1 N, the rotation speed was 0.1256 m / s, and the friction time was 30 min.
[0104] Pencil hardness Adhesion grade Contact angle (°) Friction coefficient Example 1 2H Level 1 142.5 0.056 Example 2 2H Level 0 145.2 0.051 Example 3 3H Level 0 146.7 0.045 Comparative Example 1 H Level 1 138.0 0.073 Comparative Example 2 HB Level 2 130.1 0.089 Comparative Example 3 B Level 2 113.9 0.097
[0105] According to the data in the above table, we can clearly draw the following conclusions:
[0106] The injection molds obtained in Examples 1-3 are compared with the injection molds obtained in Comparative Examples 1-3. The test results show that:
[0107] Compared with the comparative example, the injection molds obtained in Examples 1-3 have better pencil hardness, adhesion level, contact angle, and lower friction coefficient data; this fully demonstrates that the present invention achieves improvements in the hardness, wear resistance, and anti-sticking properties of the injection mold coating.
[0108] Compared with Example 1, the fillers in Comparative Example 1 are graphene and molybdenum disulfide; the fillers in Comparative Example 2 are graphene and molybdenum disulfide, and the polyphenylene sulfide modification process is different; the filler in Comparative Example 3 is graphene, and the polyphenylene sulfide is not modified. The injection molds obtained in Comparative Examples 1-3 have deteriorated pencil hardness, adhesion grade, contact angle, and friction coefficient data. It can be seen that the configuration, compounding and modification of the filler components, the modification of polyphenylene sulfide and the setting of the components used in the present invention can promote the improvement of the hardness, wear resistance and anti-sticking properties of the coating of the prepared injection mold.
[0109] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process method article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process method article or device.
[0110] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing an injection mold having a high hardness and wear-resistant coating, Features: Including the following processes: Spraying the coating on the mold surface, drying, sintering, forming a coating, and obtaining an injection mold; The coating comprises the following components by mass: 65 to 85 parts of polytetrafluoroethylene, 15 to 20 parts of modified polyphenylene sulfide, 9.1 to 15.0 parts of modified filler, 1.4 to 2.0 parts of auxiliary agent, and 260 to 338 parts of solvent; The specific preparation process of the modified polyphenylene sulfide is as follows: Take polyphenylene sulfide, p-chloroaniline, sodium hydroxide and 1-methyl-pyrrolidone and mix them. Under the protection of nitrogen atmosphere, heat them to 245-255° C. and keep them warm for 180-220 min; cool them to 215-225° C. and keep them warm for 18-24 min; cool them to 120-140° C. to obtain amino-terminated polyphenylene sulfide; The amino-terminated polyphenylene sulfide is mixed with aniline, 2-fluoroaniline, ammonium persulfate and sulfuric acid solution at 0-2°C, placed in an autoclave, and reacted for 4-7 hours at a temperature of 3-5°C and a pressure of 0.1-1.0 MPa to obtain modified polyphenylene sulfide; The specific preparation process of the modified filler is: Mix KH560 and ethanol solution, heat to 60-70°C and stir for 7-12 minutes, add filler, and continue stirring for 60-90 minutes; cool, centrifuge, and wash to obtain modified filler; The filler comprises the following mass components: 5 to 6 parts of graphene, 3 to 6 parts of composite graphene, and 1.1 to 3.0 parts of molybdenum disulfide; The specific preparation process of the composite graphene is as follows: The graphene is dispersed in deionized water, polyvinyl pyrrolidone is added, ethanol and sodium citrate dihydrate are added in sequence and mixed evenly, ammonia water and ethyl orthosilicate are added, the temperature is raised to 88-94° C. and the mixture is reacted for 120-180 minutes; the mixture is filtered and washed to obtain composite graphene.
2. A method for preparing an injection mold having a high hardness and wear-resistant coating according to claim 1, Features: The mass ratio of polyphenylene sulfide, p-chloroaniline and sodium hydroxide is 24: (0.5-0.6): (0.7-0.8); The ratio of amino-terminated polyphenylene sulfide, aniline, 2-fluoroaniline, ammonium persulfate, and sulfuric acid solution is 20 g: (0.25-0.46) g: (0.28-0.55) g: (1.3-2.4) g: 100 mL.
3. A method for preparing an injection mold having a high hardness and wear-resistant coating according to claim 1, Features: The mass ratio of the graphene, polyvinyl pyrrolidone, sodium citrate dihydrate and tetraethyl orthosilicate is 5: (5.6-11.3): (0.04-0.08): (0.5-1.0).
4. The method for preparing an injection mold having a high hardness and wear-resistant coating according to claim 1, Features: The spraying process conditions are: spraying pressure 0.2-0.3 MPa, nozzle diameter 1.8 mm, distance between nozzle and mold 200-250 mm, spraying rate 6-8 m / min; The spraying thickness is 20-40 μm.
5. The method for preparing an injection mold having a high hardness and wear-resistant coating according to claim 1, Features: The sintering process conditions are: 280-290° C., baking and heat preservation for 75-100 minutes; 360-380° C., curing and heat preservation for 12-18 minutes, and cooling with the furnace.
6. A wear-resistant coating with high hardness obtained according to the preparation method according to any one of claims 1 to 5.
Citation Information
Patent Citations
Preparation method of coating of grapheme modified polyphenylene sulfide
CN106479296A
Paint for automobile coating
CN110128913A