Preparation method of pre-lithiation binder and silicon-carbon electrode for silicon-carbon power battery
By prelithiating the three-dimensional adhesive, an efficient silicon carbon electrode adhesive was prepared, which solved the problem of silicon-based anode volume expansion and low ICE, and significantly improved the initial Coulomb efficiency and cycling performance of the electrode. Suitable for industrial applications.
Patent Information
- Application Number
- CN202311131682.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-04
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-09-04
AI Technical Summary
Due to the problems of volume expansion and low initial Coulomb efficiency (ICE) in lithium-ion batteries, the existing technology is difficult to effectively alleviate, affecting its commercial application.
Prelithiation of three-dimensional binder by using three-dimensional three-dimensional binder, and the three-dimensional crosslinked polymer binder is prepared by condensation reaction between polyacrylic acid (PAA) and lithium carboxymethylcellulose, which improves the viscosity and mechanical strength of the binder and enhances the The migration ability of lithium ions is combined with the prelithiation of CMC-Li to form an efficient prelithiated binder.
It significantly improves the initial Coulomb efficiency and cyclic performance of silicon carbon electrodes, enhances the integrity and long-term stability of the electrodes, and is suitable for large-scale industrial operations.
Smart Images

Figure CN117165227B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium batteries, and in particular to a method for preparing a pre-lithiation binder and a silicon-carbon electrode for a silicon-carbon power battery. Background Art
[0002] Since the first commercialization of lithium-ion batteries (LIBs) in 1991, LIBs have made significant progress and become the main power source for various portable electronic devices and electric vehicles. In addition, as an efficient energy storage technology with relatively high energy density and long cycle life, LIBs also play a vital role in addressing global climate issues and promoting global sustainable development. Graphite, as a commonly used traditional anode material, is currently the material of choice due to its high capacity retention, low volume change (10%), low cost and low toxicity. However, the energy density of LIBs is limited by the maximum specific capacity of graphite (372mA h / g), which can no longer meet daily needs.
[0003] Silicon-based materials have high theoretical capacity and have been recognized by academia and industry as the most promising anodes for high-energy density lithium-ion batteries (LIBs). However, based on the alloying / de-alloying mechanism, the volume of silicon-based anodes changes greatly (>300%) during the lithiation / de-lithiation process, exposing silicon particles to mechanical fatigue, resulting in electrode pulverization and instability of the solid electrolyte interface (SEI). According to the view that the reaction mechanism and some side reactions of silicon-based anodes will form SEI during the initial cycle, silicon-based anodes will consume Li+ to form SEI and undergo some side reactions in the first few electrochemical cycles, which means that silicon-based anodes have low initial coulombic efficiency (ICE) or require additional cathode materials to supplement the low ICE of the anode material. Solving the volume expansion and low ICE problems of silicon-based anodes is of great significance to promoting the commercialization of silicon-based materials.
[0004] Binder is one of the key components in the electrode. It can combine active materials and conductive additives on the current collector and maintain the integrity of the electrode during the charge and discharge process of the battery. There are literature reports on the fact that different binders can alleviate the volume change of silicon-based anodes. According to the development history of binders for silicon-based materials in recent years, binders have gradually evolved from PVDF, which was originally connected to the material only by weak intermolecular forces, to functional polymer binders containing certain special functional groups, such as PAA, CMC, etc., and to three-dimensional binders that have attracted much attention in recent years. According to existing literature records, three-dimensional binders are most effective in alleviating the volume expansion of silicon-based materials, but they are not very effective in improving the ICE of silicon-based materials. Therefore, it is of great significance to design a multifunctional binder that can effectively alleviate the volume expansion of silicon-based materials and improve their ICE. Summary of the invention
[0005] The purpose of the present invention is to overcome the defects of the prior art and provide a method for preparing a pre-lithiation binder and a silicon-carbon electrode for a silicon-carbon power battery.
[0006] The present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing a pre-lithiation binder for a silicon-carbon power battery, comprising the following steps:
[0008] S1. preparing lithium carboxymethyl cellulose;
[0009] S2. Pre-lithiation of polyacrylic acid: Take a certain amount of polyacrylic acid powder, add an appropriate amount of deionized water and stir to prepare a polyacrylic acid solution. Add a certain amount of LiOH to the polyacrylic acid solution, and after acid-base reaction, obtain PAA-Li x Solution;
[0010] S3, dissolve lithium carboxymethyl cellulose in deionized water to prepare lithium carboxymethyl cellulose solution, and x The solution and the lithium carboxymethyl cellulose solution are mixed and stirred in a ratio of 9:1 to obtain the pre-lithiation binder;
[0011] In step S2, the molar ratio of polyacrylic acid to LiOH is 1:0.5-1, and x=0.5-1.
[0012] Pre-lithiation is an excellent method to improve the ICE of silicon-based materials. Pre-lithiation is a method of supplementing additional lithium sources to improve ICE and alleviate the initial loss of active lithium. However, the methods for pre-lithiation of silicon-based anodes in the prior art are direct electrochemical pre-lithiation of the silicon-based anode, chemical pre-lithiation, and direct covering of the electrode surface with lithium foil / lithium source (and subsequent physical activation). Pre-lithiation methods from the perspective of binders are not considered, or only a single type of binder is pre-lithiated.
[0013] The present invention uses a three-dimensional binder containing special groups as a framework, performs pre-lithiation on it, and seeks the best pre-lithiation degree to alleviate the volume expansion problem of silicon-based materials while improving their ICE.
[0014] Furthermore, in step S2, the molar ratio of polyacrylic acid to LiOH is 1:0.75, and x=0.75.
[0015] Further, in step S3, the lithium carboxymethyl cellulose solution and the PAA-Li x The mass fraction of the solution is 4%.
[0016] If the concentration of the main component in the binder is too low, the bonding effect is poor, and if the concentration is too high, the slurry will thicken and the electrode performance will be poor. Therefore, the carboxymethyl cellulose lithium solution and PAA-Li x The mass concentration of the solution is selected to be 4%.
[0017] Further, the steps of preparing lithium carboxymethyl cellulose are:
[0018] S11, dissolving carboxymethyl cellulose in 95% ethanol to obtain a suspension, adding HCl solution to the suspension and stirring at room temperature, filtering, washing, and vacuum drying overnight to obtain a white powder;
[0019] S12. Ultrasonic dispersion of the white powder in 75% ethanol, adding LiOH aqueous solution under vigorous stirring, reacting under stirring in a 50°C water bath, washing with anhydrous ethanol after natural cooling, and vacuum drying overnight to obtain lithium carboxymethyl cellulose.
[0020] The present invention also provides a pre-lithiation binder for a silicon-carbon power battery obtained by the above preparation method.
[0021] The present invention also provides a silicon-carbon electrode, comprising a silicon-carbon active material, a conductive aid and the above-mentioned pre-lithiation binder, wherein the mass ratio of the silicon-carbon active material, the conductive aid and the pre-lithiation binder is 7:2:1.
[0022] The present invention also provides a method for preparing the silicon-carbon electrode, comprising the steps of:
[0023] S1. Mixing the silicon-carbon active material, the conductive additive and the pre-lithiation binder in deionized water in a mass ratio of 7:2:1 to obtain a uniform slurry;
[0024] S2. The slurry is coated on a copper foil to form a film, and the silicon-carbon electrode is obtained after drying.
[0025] Furthermore, the drying is carried out in a vacuum oven at 150° C. for 2 h.
[0026] Technical principle of the present invention:
[0027] CMC is carboxymethyl cellulose, while CMC-H is insoluble in water. CMC is pre-lithiated to remove Na + The second is to improve its solubility;
[0028] Pre-lithiation of PAA can first improve the PAA-Li x The viscosity of the solution and the prepared mixed binder, according to the results, shows that the viscosity of the binder will increase after pre-lithiation. This is because after pre-lithiation, the long chains stretch out and the interchain entanglement strength increases, which increases the viscosity of the binder after pre-lithiation, and the higher the degree of pre-lithiation, the greater the viscosity. At the same time, the mechanical strength of the interchain entanglement increases when the long chains stretch out, which is beneficial to maintaining the integrity of the electrode and improving the long-term stability of the battery. In addition, during the coating process, under low viscosity conditions, the active materials and conductive particles tend to settle quickly, while under high viscosity conditions, the active materials and conductive particles cannot be effectively separated.
[0029] Moreover, the pre-lithiation of PAA and the pre-reaction of LiOH with -COOH in PAA can reduce the side reactions in the reaction; at the same time, the pre-lithiation of the binder can increase the ionic conductivity. With the creeping movement of the binder chain, Li + Can be transferred to -COOH, greatly promoting the migration of lithium ions;
[0030] Finally through Li x The condensation reaction of PAA and CMC-Li is used to prepare a three-dimensional cross-linked polymer adhesive. Different degrees of pre-lithiation of PAA can be used to screen out the viscosity that is most conducive to large-scale industrial operations.
[0031] The present invention has the following beneficial effects:
[0032] The present invention uses the unique groups of the three-dimensional binder to perform systematic pre-lithiation, and uses PAA-Li xA three-dimensional cross-linked polymer binder was prepared by condensation reaction with CMC-Li. By pre-lithiation of PAA to different degrees, the viscosity that is most conducive to large-scale industrial operation was screened out, while ensuring its good mechanical properties, the ICE and cycle performance of the silicon-carbon electrode were improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0034] Figure 1 It is a reaction principle diagram of an embodiment of the present invention;
[0035] Figure 2 This is an infrared comparative analysis diagram of the adhesives prepared in Examples 1 to 5 of the present invention;
[0036] Figure 3 The SEM images of silicon-carbon electrodes prepared by the binders of Examples 1, 2 and 4 of the present invention;
[0037] Figure 4 The initial charge and discharge curves of the silicon-carbon electrodes prepared in Examples 6 to 10 of the present invention at 0.1 A / g;
[0038] Figure 5 The initial coulomb efficiency diagram of the silicon-carbon electrode prepared in Examples 6 to 10 of the present invention at 0.1 A / g;
[0039] Figure 6 The cycle curves of the silicon carbon electrodes prepared in Examples 6 to 10 of the present invention at 0.2 A / g;
[0040] Figure 7 The cycle curves of the silicon-carbon electrodes prepared in Examples 6 to 10 of the present invention at 0.5 A / g;
[0041] Figure 8 This is a rate performance diagram of the silicon-carbon electrodes prepared in Examples 6 to 10 of the present invention. DETAILED DESCRIPTION
[0042] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0043] An embodiment of the present invention provides a method for preparing a pre-lithiation binder for a silicon-carbon power battery, comprising the following steps:
[0044] S1. preparing lithium carboxymethyl cellulose;
[0045] S2. Pre-lithiation of polyacrylic acid: Take a certain amount of polyacrylic acid powder, add an appropriate amount of deionized water and stir to prepare a polyacrylic acid solution. Add a certain amount of LiOH to the polyacrylic acid solution, and after acid-base reaction, obtain PAA-Li x Solution;
[0046] S3, dissolve lithium carboxymethyl cellulose in deionized water to prepare lithium carboxymethyl cellulose solution, and x The solution and the lithium carboxymethyl cellulose solution are mixed and stirred in a ratio of 9:1 to obtain the pre-lithiation binder;
[0047] In step S2, the molar ratio of polyacrylic acid to LiOH is 1:0.5-1, and x=0.5-1.
[0048] The present invention is through PAA-Li x Preparation of three-dimensional cross-linked polymer binder, PAA-Li by condensation reaction (dehydration) with CMC-Li x The carboxylic acid group of CMC-Li reacts with the hydroxyl group of CMC-Li under vacuum at 150℃ to obtain ester groups through interchain crosslinking, effectively forming a crosslinked structure. The specific reaction principle diagram is shown in Figure 1 By pre-lithiation of PAA to different degrees, the viscosity that is most conducive to large-scale industrial operation was screened out. Finally, it was found that when the molar ratio of polyacrylic acid and LiOH was 1:0.5~1 and x=0.5~1, the silicon-carbon electrode had a large ICE and good cycling performance.
[0049] As a preferred embodiment, the molar ratio of polyacrylic acid to LiOH is 1:0.75, and x=0.75.
[0050] As a preferred embodiment, in step S3, the lithium carboxymethyl cellulose solution and the PAA-Li x The mass fraction of the solution is 4%.
[0051] The preparation of lithium carboxymethyl cellulose is specifically as follows:
[0052] S11, dissolving carboxymethyl cellulose in 95% ethanol to obtain a suspension, adding HCl solution to the suspension and stirring at room temperature for 2 hours, filtering, washing, and vacuum drying overnight to obtain a white powder;
[0053] S12. Ultrasonic dispersion of the white powder in 75% ethanol, adding LiOH aqueous solution under vigorous stirring, reacting under stirring in a 50°C water bath, washing with anhydrous ethanol after natural cooling, and vacuum drying overnight to obtain lithium carboxymethyl cellulose.
[0054] An embodiment of the present invention further provides a silicon-carbon electrode, comprising a silicon-carbon active material, a conductive aid and the pre-lithiation binder prepared as above, wherein the mass ratio of the silicon-carbon active material, the conductive aid and the pre-lithiation binder is 7:2:1.
[0055] The present invention also provides a method for preparing the silicon-carbon electrode, comprising the steps of:
[0056] S1. Mixing the silicon-carbon active material, the conductive additive and the pre-lithiation binder in deionized water in a mass ratio of 7:2:1 to obtain a uniform slurry;
[0057] S2. The slurry is coated on a copper foil to form a film, and the silicon-carbon electrode is obtained after drying.
[0058] In a specific embodiment, the drying is carried out in a vacuum oven at 150° C. for 2 h.
[0059] Examples 1 to 5
[0060] The pre-lithiation binder is prepared as follows:
[0061] 1. Preparation of CMC-Li: 10g CMC was dissolved in 150mL 95% ethanol and stirred for 30min to obtain suspension A. Then, 20mL 6mol / L HCl solution was slowly added to suspension A and stirred at room temperature for 2h, filtered and washed with 75% ethanol and anhydrous ethanol for 3 times, and kept in vacuum at 80℃ overnight to obtain white powder B. 3.7g white powder B was ultrasonically dispersed in 45mL 75% ethanol, and then 15mL aqueous solution containing 1.02g LiOH was added under vigorous stirring, and reacted under stirring at 50℃ water for 2h, cooled naturally to room temperature, washed with anhydrous ethanol several times, and kept in vacuum at 80℃ overnight to obtain the desired white powder CMC-Li.
[0062] 2. Pre-lithiation of PAA: Under normal temperature, take a certain mass of PAA powder and add an appropriate amount of deionized water, stir overnight, and prepare a solution A with a mass concentration of 4%. Add a certain mass of LiOH solid to solution A, where the mass of LiOH solid is determined according to the molar amount of -COOH contained in PAA and the pre-lithiation degree x (x = 0, 0.25, 0.50, 0.75, 1). After acid-base reaction, a PAA-Li with a mass fraction of 4% is obtained. x(x=0, 0.25, 0.50, 0.75, 1) solution, so as to achieve the purpose of pre-lithiation of polyacrylic acid
[0063] 3. Preparation of pre-lithiation binder: Under room temperature, a certain amount of the prepared carboxymethyl cellulose lithium was dissolved in deionized water and stirred overnight to prepare a CMC-Li solution with a mass fraction of 4%. x The solution and the CMC-Li solution were mixed in a mass ratio of 9:1 and stirred for a period of time to prepare a pre-lithiation binder with a mass fraction of 4%.
[0064] According to PAA-Li x The values of x are different, and the binders are denoted as CL-PL0, CL-PL 0.25 ,CL-PL 0.50 ,CL-PL 0.75 and CL-PL 1.00 The binder prepared in Example 1 is CL-PL0, and the binder prepared in Example 2 is CL-PL 0.25 The binder prepared in Example 3 is CL-PL 0.50 The binder prepared in Example 4 is CL-PL 0.75 The binder prepared in Example 5 is CL-PL 1.00 .
[0065] Embodiments 6 to 10
[0066] The pre-lithiation binder prepared in Examples 1 to 5 was used to prepare Si / C electrodes. The preparation process of the Si / C electrode was as follows: the active material (Si / C), the conductive additive (superP) and the pre-lithiation binder were mixed in deionized water at a mass ratio of 7:2:1 to obtain a uniform slurry. The slurry was then applied to a copper foil, and a 150 μm medical scalpel was used to apply a flat and smooth film, which was dried in a vacuum oven at 150°C for 2 hours and cut into a circular Si / C electrode with a radius of 8 mm.
[0067] Test Example 1
[0068] The adhesives prepared in Examples 1 to 5 were subjected to infrared diffraction analysis, and the results are shown in Figure 2 As can be seen from the figure, at 1369cm -1 There is a characteristic peak at 1395-1467cm -1 There is a characteristic peak band at the - ), it can be concluded that the system contains Li + More importantly, the C=O stretching peak in the carboxyl group is from 1703 cm -1 Offset to 1723cm -1The characteristic peak of anhydride is located at 1805 cm -1 It can be judged that the characteristic peak is caused by the formation of ester group (COO). Another characteristic peak band is 1166-1322cm -1 The corresponding chemical bond is COC. Combined with this point, it can be concluded that after heating treatment, an ester group is formed in the internal structure of the adhesive, which is consistent with the proposed reaction principle.
[0069] Test Example 2
[0070] The electrodes prepared by the binders of Example 1, Example 2 and Example 4 were analyzed by scanning electron microscope. Figure 3 When CL-PL0 adhesive was used, the surface had several protrusions and many deep cracks (as shown in a in the figure); compared with the SEM image of CL-PL0 adhesive, when CL-PL 0.25 When the binder is used, there are many protrusions and cracks on the electrode surface, which is obviously more than that in Figure a (as shown in Figure b); while when CL-PL 0.75 When the binder is added, the electrode surface is relatively smooth, with only a few small cracks (as shown in c in the figure).
[0071] This is due to the difference in the dispersion and bonding of Si / C particles by the binder in actual situations. Analyzing from the connection mode between the binder and the surface of Si particles, it mainly relies on the condensation reaction between the free carboxylic acid of PAA and the hydroxyl group of the silica layer on the silicon surface to form a covalent ester bond and partial hydrogen bond between the binder and the silicon particles, thereby achieving the bonding of the binder and Si / C particles and alleviating the volume expansion problem of Si / C materials. In addition, partial pre-lithiation of the binder can gradually make the polymer chain present a stretched conformation, and the contact sites between the binder and the active material increase, and through the interaction of hydrogen bonds and chemical bonds, it will have a strong interface adhesion with the active material. CL-PL 0.25 Compared with CL-PL0 adhesive, CL-PL 0.25 The contact sites between the binder and the active material are increased, but the number of -COOH is less than that of the CL-PL0 binder, which is not conducive to the dispersion and connection of the active material, resulting in many protrusions and cracks on the electrode surface. 0.75 Due to the high degree of pre-lithiation of the binder, the polymer chain of the binder is almost completely stretched, with more contact sites with the active material and stronger interaction with the active material. In addition, its high viscosity is conducive to the dispersion of the active material. For the above reasons, when using CL-PL 0.25 When using the binder, there are many protrusions and cracks on the electrode surface. Use CL-PL 0.75 The surface of the adhesive is smooth and has only a few small cracks.
[0072] Test Example 3
[0073] The circular Si / C electrodes prepared in Examples 6 to 10 were respectively made into 2025 type coin batteries. The specific operation was as follows: in a glove box filled with argon, the batteries were assembled under the condition that the water and oxygen content was less than 0.1 ppm, wherein the electrolyte used for assembling the batteries was 1M LiPF6 in EC / DMC / EMC (1:1:1 v / v / v) and an appropriate amount of additive FEC (volume fraction of 10%) was added.
[0074] The constant current charge and discharge cycle test was carried out using the Neware battery test system: the Si / C half-cell was tested between 0.01-3.0V and activated for 3 cycles at 0.1A / g to obtain the cycle curves and rate curves at 0.2A / g and 0.5A / g.
[0075] from Figure 4 , 5 The results show that CL-PL 0.50 ,CL-PL 0.75 and CL-PL 1.00 Effectively improve the ICE of silicon carbon electrode, among which CL-PL 0.75 for the best;
[0076] from Figure 6 , 7 It can be seen from the cycle curve that the prepared silicon carbon electrodes have high coulombic efficiency; Figure 8 It can be seen that when the test current first increases to 2 A / g and then recovers to 0.1 A / g, the discharge capacity of the battery can be restored to the initial level.
[0077] The present invention uses the unique groups of the three-dimensional binder to perform systematic pre-lithiation, and uses PAA-Li x The three-dimensional cross-linked polymer binder was prepared by condensation reaction of PAA and CMC-Li. The viscosity that is most conducive to large-scale industrial operation was screened out by pre-lithiation of PAA to different degrees. While ensuring its good mechanical properties, the ICE and cycle performance of the silicon carbon electrode were improved. 0.75 The best, with the best ICE and cycle performance.
[0078] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a pre-lithiation binder for a silicon-carbon power battery, characterized in that: The following steps are involved: S1. preparing lithium carboxymethyl cellulose; S2. Pre-lithiation of polyacrylic acid: Take a certain amount of polyacrylic acid powder, add an appropriate amount of deionized water and stir to prepare a polyacrylic acid solution. Add a certain amount of LiOH to the polyacrylic acid solution, and after acid-base reaction, obtain PAA-Li x Solution; S3, dissolve lithium carboxymethyl cellulose in deionized water to prepare lithium carboxymethyl cellulose solution, and x The solution and the lithium carboxymethyl cellulose solution are mixed and stirred in a ratio of 9:1 to obtain the pre-lithiation binder; In step S2, the molar ratio of polyacrylic acid to LiOH is 1:0.75, x=0.75; In step S3, the lithium carboxymethyl cellulose solution and PAA-Li x The mass fraction of the solution is 4%; The steps for preparing lithium carboxymethyl cellulose are: S11, dissolving carboxymethyl cellulose in 95% ethanol to obtain a suspension, adding HCl solution to the suspension and stirring at room temperature, filtering, washing, and vacuum drying overnight to obtain a white powder; S12. Ultrasonic dispersion of the white powder in 75% ethanol, adding LiOH aqueous solution under vigorous stirring, reacting under stirring in a 50°C water bath, washing with anhydrous ethanol after natural cooling, and vacuum drying overnight to obtain lithium carboxymethyl cellulose.
2. A pre-lithiation binder for a silicon-carbon power battery prepared by the preparation method of a pre-lithiation binder for a silicon-carbon power battery according to claim 1.
3. A silicon-carbon electrode, characterized in that: The invention comprises a silicon-carbon active material, a conductive additive and the pre-lithiation binder according to claim 2, wherein the mass ratio of the silicon-carbon active material, the conductive additive and the pre-lithiation binder is 7:2:
1.
4. The method for preparing the silicon-carbon electrode according to claim 3, characterized in that: Includes steps: S1. Mixing the silicon-carbon active material, the conductive additive and the pre-lithiation binder in deionized water in a mass ratio of 7:2:1 to obtain a uniform slurry; S2. The slurry is coated on a copper foil to form a film, and the silicon-carbon electrode is obtained after drying.
5. The method for preparing a silicon-carbon electrode according to claim 4, characterized in that: The drying is carried out in a vacuum oven at 150° C. for 2 h.
Citation Information
Patent Citations
Aqueous composite binder and method for preparing aqueous positive electrode slurry therefrom
CN105153974A
Electrode material slurry and secondary battery comprising the same
CN109473626A
Negative electrode material binder for low-temperature lithium ion battery, negative electrode material, negative electrode plate and preparation method
CN115360350A
High capacity anode electrodes with mixed binders for energy storage devices
US20180261881A1
Composite binder for lithium ion batteries and its preparation
WO2018227366A1