A method for preparing temperature-controlled precipitation chloride molten salt purification
The water and oxygen impurities in the molten salt of chloride were removed by temperature control and sedimentation method, and the problems of impurities introduction, high cost and high energy consumption in the existing molten salt purification methods of chloride were solved, thus achieving high efficiency and low cost purification effect, improving the The stability and heat storage properties of molten salts are achieved.
Patent Information
- Application Number
- CN202310964239.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-01
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-08-01
AI Technical Summary
The existing chloride molten salt purification methods have problems such as introduction of impurities, high cost, large energy consumption, and poor purification effect on active metal ions, especially in large-scale processing, which is difficult to achieve efficient purification.
Through the temperature-controlled sedimentation method, alkaline aluminum chloride is formed by reacting aluminum chloride with water and oxygen, reducing the melting temperature to agglomerate and settle, thereby realizing solid-liquid separation, removing water and oxygen impurities, avoiding high-temperature decomposition, and simplifying the purification process.
It effectively reduces the corrosiveness of molten salt, improves stability and heat storage performance, is simple to operate and low cost, is suitable for large-scale processing, avoiding the introduction of impurities and high energy consumption.
Smart Images

Figure CN117185330B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of molten salt, and in particular relates to a method for preparing temperature-controlled precipitation chloride molten salt purification. Background Art
[0002] Among various heat transfer and heat storage media, molten salt has become the most potential high-efficiency medium and high temperature heat transfer and storage medium due to its low viscosity, wide operating temperature range, high heat transfer performance, and strong heat storage capacity. Chloride molten salt has the advantages of high thermal conductivity, wide operating temperature range, low viscosity, and low cost, and is the focus of future high-temperature heat transfer and thermal storage material development.
[0003] The main challenge in the application of chloride molten salt is compatibility with structural materials, usually high-temperature alloys or stainless steel. Since the intrinsic corrosion of high-purity chloride molten salt is very small, impurities such as water or oxides play an important role in the metal corrosion mechanism of molten salt. In addition, impurities such as water and oxygen will also form oxide precipitation with metals, causing changes in the composition of the molten salt and reducing the stability and heat storage performance of the molten salt.
[0004] At present, the main methods used for molten salt purification are the introduction of HX-H2 (X is a halogen), electrochemical purification methods, and the addition of metal reducing agents. However, halogenated hydrocarbon gases are highly corrosive to chloride molten salts, and they need to be completely removed after purification, which is difficult and costly. The electrochemical purification method has high requirements for the purity of the solvent, consumes a lot of chemical raw materials and energy, and has a poor purification effect on the active metal ions of chloride molten salts. For example: CN201811057800.1 A method for preparing a high-purity chloride molten salt and its application, the active metal includes at least one of lithium, potassium, calcium, sodium, magnesium, aluminum, zinc and iron, and the active metal reacts with oxidizing impurities for reduction. First of all, the cost is high, the reaction safety is low, and the addition of a metal reducing agent is easy to introduce new impurities, and there are high requirements for the purity of the metal reducing agent.
[0005] Therefore, a method is needed that does not introduce impurities, has low material and energy consumption, has good purification effect, and is suitable for large-scale treatment and purification of chloride molten salt. Summary of the invention
[0006] The present invention aims to provide a method for purifying molten salt containing chloride by temperature-controlled precipitation, which is based on the characteristics of molten salt containing aluminum chloride, that is, aluminum chloride, the main component of molten salt in liquid molten salt, will react with water oxygen (such as H2O, OH) at a certain temperature. - The solid aluminum chloride is formed by lowering the melting temperature to prevent the decomposition of the basic aluminum chloride at high temperature, so that it has sufficient time to agglomerate and settle, thereby removing the water and oxygen impurities through simple solid-liquid separation.
[0007] As an excellent heat transfer medium, the metal corrosion of chloride molten salt is the most important factor determining whether it can be used in engineering. This method removes impurities in the molten salt by cooling and sedimentation, which greatly reduces the water and oxides in the molten salt, reduces the corrosion of the molten salt to metals, and improves the stability and heat storage performance of the molten salt.
[0008] The technical purpose of the present invention is achieved through the following technical solutions:
[0009] Step 1: The chloride raw material powder containing aluminum chloride is mixed evenly according to the proportion to obtain a white solid powder. The chloride containing aluminum chloride is a mixture of one or more of sodium chloride, potassium chloride, lithium chloride, and zinc chloride with aluminum chloride. The mass of aluminum chloride accounts for ≥30.0% of the total chloride. The purity of the chloride raw material used is
[0010] ≥99.0%, moisture content ≤1.0%.
[0011] Step 2: Pour the white solid powder obtained in step 1 into a crucible, place it in a heating furnace, heat it to 150-200°C and sinter it for 0.5-2h to melt the white solid into liquid.
[0012] Step 3: After the solid melts, heat it up to 200-450°C and keep it constant for 0.1-1h, and a black solid will form in the liquid. Step 4: Cool the liquid to below 200°C and keep it constant to allow the black solid to settle.
[0013] Step 5: After the black solid has settled, separate the upper layer of liquid molten salt while it is still hot.
[0014] Step 6: The liquid molten salt is cooled to obtain purified solid molten salt.
[0015] All of the above steps 1-6 are completed under a protective atmosphere, and the protective gas is high-purity nitrogen or argon.
[0016] The molten salt purification method provided by the present invention first heats the chloride molten salt raw material to turn it into liquid. The liquid can accelerate the reaction of aluminum chloride with water on the one hand, and can be well separated from the solid generated by the reaction on the other hand. When the temperature rises to above 200°C, aluminum chloride reacts with water oxygen to form basic aluminum chloride. To prevent basic aluminum chloride from decomposing at high temperature for a long time, the temperature needs to be lowered to below 200°C. Basic aluminum chloride forms polymers, which agglomerate and settle for separation and removal.
[0017] Advantages of the present invention: The present invention does not require the addition of reducing gas, active metal or reducing agent, does not introduce new impurities, and only controls the melting temperature of the molten salt to remove oxygen impurities in the molten salt water, thereby achieving the purpose of molten salt purification. The method of the present invention is simple to operate, low in cost, and easy to produce and apply. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 DSC curves of samples 1, 2 and 3. DETAILED DESCRIPTION
[0019] The following is a detailed description of the method for purifying molten chloride salt by temperature-controlled precipitation using a specific chloride molten salt in combination with an embodiment. All operations in the following embodiments are performed in a glove box, and the protective gas is high-purity nitrogen.
[0020] Embodiment 1:
[0021] Step 1: Weigh 24.69 g of sodium chloride, 10.48 g of potassium chloride and 67.83 g of aluminum chloride, and mix and grind the three chlorides evenly.
[0022] Step 2: Pour the white solid powder obtained in step 1 into a crucible, place it in a heating furnace, heat it to 160°C and burn it for 1 hour to melt the white solid into liquid.
[0023] Step 3: After the solid melts, the temperature is raised to 300°C and kept constant for 1 hour, and a black solid is formed in the liquid.
[0024] Step 4: Cool the liquid to 160°C and maintain the constant temperature for 5 hours to allow the black solid to settle.
[0025] Step 5: After the black solid has completely settled, pour out the upper clear liquid molten salt while it is still hot.
[0026] Step 6: The liquid molten salt is cooled to obtain a white solid molten salt, which is sample 1. The components of the white solid molten salt are sodium chloride, potassium chloride and aluminum chloride. Since the moisture content of the chloride raw material is very low (≤1.0%), very little aluminum chloride is lost during the impurity removal process.
[0027] Embodiment 2:
[0028] Step 1: Weigh 24.69 g of sodium chloride, 10.48 g of potassium chloride and 67.83 g of aluminum chloride, and mix and grind the three chlorides evenly.
[0029] Step 2: Pour the white solid powder obtained in step 1 into a crucible, place it in a heating furnace, raise the temperature to 200°C and keep it constant for 1 hour to melt the white solid into liquid.
[0030] Step 3: After the solid melts, the temperature is raised to 450°C and kept constant for 0.5 hours, and a black solid is formed in the liquid.
[0031] Step 4: Cool the liquid to 150°C and maintain the constant temperature for 3 hours to allow the black solid to settle.
[0032] Step 5: After the black solid has completely settled, pour out the upper clear liquid molten salt while it is still hot.
[0033] Step 6: The liquid molten salt is cooled to obtain white solid molten salt, which is sample 2.
[0034] Embodiment 3:
[0035] Step 1: Weigh 28.75 g of sodium chloride and 65.25 g of aluminum chloride, and mix and grind the two chlorides evenly.
[0036] Step 2: Pour the white solid powder obtained in step 1 into a crucible, place it in a heating furnace, raise the temperature to 150°C, and burn at a constant temperature for 1 hour to melt the white solid into liquid.
[0037] Step 3: After the solid melts, the temperature is raised to 350°C and kept constant for 1 hour, and a black solid is formed in the liquid.
[0038] Step 4: Cool the liquid to 140°C and maintain the constant temperature for 3 hours to allow the black solid to settle.
[0039] Step 5: After the black solid has completely settled, pour out the upper clear liquid molten salt while it is still hot.
[0040] Step 6: The liquid molten salt is cooled to obtain white solid molten salt, which is sample 3.
[0041] Comparative Example 1:
[0042] Step 1: Weigh 24.69 g of sodium chloride, 10.48 g of potassium chloride and 67.83 g of aluminum chloride, and mix and grind the three chlorides evenly.
[0043] Step 2: Pour the white solid powder obtained in step 1 into a crucible, place it in a heating furnace, heat it to 160°C and burn it for 1 hour to melt the white solid into liquid.
[0044] Step 3: After the solid melts, the temperature is raised to 450°C and kept constant for 3 hours. A black solid forms in the liquid and settles.
[0045] Step 4: After the black solid has completely settled, pour out the upper layer of liquid molten salt while it is still hot.
[0046] Step 5: The liquid molten salt is cooled to obtain a white solid molten salt, which is comparison sample 1.
[0047] Comparative Example 2:
[0048] Step 1: Weigh 24.69 g of sodium chloride, 10.48 g of potassium chloride and 67.83 g of aluminum chloride, and mix and grind the three chlorides evenly.
[0049] Step 2: Pour the white solid powder obtained in step 1 into a crucible, place it in a heating furnace, heat it to 160°C and burn it for 1 hour to melt the white solid into liquid.
[0050] Step 3: Maintain constant temperature at 160°C for 4 hours.
[0051] Step 4: The liquid molten salt is cooled to obtain an off-white solid molten salt, which is comparison sample 2.
[0052] The melting point of the sample was tested by differential scanning calorimetry. The differential scanning calorimeter was placed in a glove box to isolate the air. About 10 mg of the sample was weighed and placed in an alumina crucible. The scanning rate was 5 °C / min, the gas flow rate was 30 mL / min, and it was heated from room temperature to 230 °C. The test was repeated twice and the melting point of the second time was taken. The DSC test results are shown in the attached Figure 1 As shown. The oxygen content of the product was analyzed and tested using a leco oxygen and nitrogen analyzer. The test results are listed in Table 1.
[0053] Table 1 Melting point and oxygen content of molten salt
[0054]
[0055] Samples 1, 2, and 3 generate black solid impurities at high temperatures, cool down the impurities and remove impurities, effectively reducing the oxygen content in the molten salt to below 300ppm. Comparative sample 1 precipitates impurities at a high temperature of 450°C, causing some impurities to decompose, thereby increasing the oxygen content to more than 300ppm. Comparative sample 2 precipitates at a lower temperature of 160°C. Since it is difficult for impurity solids to form at low temperatures, it is difficult to separate subsequent impurities from the molten salt, resulting in an oxygen content of up to 7900ppm in the molten salt.
[0056] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A method for purifying chloride molten salt by temperature-controlled precipitation, characterized in that: The purification preparation method is as follows: Step 1: Pour the chloride raw material powder containing aluminum chloride into a crucible, place it in a heating furnace, and heat it to 150-200°C to melt the solid into liquid; Step 2: After the solid is melted, the temperature is raised to 200-450°C and the temperature is maintained constant until a black solid is formed in the liquid; Step 3: After step 2, cool the liquid to below 200°C and maintain a constant temperature to allow the black solid to settle; Step 4: After the black solid has settled, separate the upper layer of liquid molten salt while it is hot, and cool the liquid molten salt to obtain purified solid molten salt.
2. The temperature-controlled precipitation chloride molten salt purification method according to claim 1 is characterized in that: The chloride raw material used in step 1 has a purity of ≥99.0% and a moisture content of ≤1.0%; the chloride containing aluminum chloride is a mixture of aluminum chloride and one or more of sodium chloride, potassium chloride, lithium chloride, and zinc chloride.
3. The temperature-controlled precipitation chloride molten salt purification method according to claim 1 is characterized in that: The aluminum chloride used in step 1 accounts for ≥30.0% by mass in the raw material.
4. The temperature-controlled precipitation chloride molten salt purification method according to claim 1 is characterized in that: The prepared molten salt is a low-melting-point eutectic salt, and its melting point is lower than 150°C.
5. The temperature-controlled precipitation chloride molten salt purification method according to claim 1, characterized in that: The purification and preparation steps are all completed under a protective atmosphere, and the protective gas is high-purity nitrogen or argon.
6. The temperature-controlled precipitation chloride molten salt purification method according to claim 1, characterized in that: The oxygen content in the purified molten salt is ≤300ppm.
Citation Information
Patent Citations
Preparation method and application of high-purity chloride molten salt
CN109207128A
High-purity anhydrous aluminum chloride and process for production thereof
CN101155759A
Purification method of chloride
CN112551567A
Molten salt, electrochemical purification method of molten salt and electrochemical device
CN113603059A
PROCESS FOR PRODUCTION OF ANHYDROUS ALUMINUM CHLORIDE
DD248110A1