Multilayer nested carbon nanotube and preparation method thereof

By using a template method to prepare multilayer nested carbon nanotubes, the problem of difficulty in preparing multilayer CNTs in existing technologies has been solved, and the controllability of tube wall thickness and cavity size has been achieved, thereby improving the performance and application potential of the material.

CN117228660BActive Publication Date: 2024-11-08HENAN ACAD OF SCI CARBON MATRIX COMPOSITES RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311171846.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-12
Publication Date
2024-11-08
Estimated Expiration
2043-09-12

AI Technical Summary

Technical Problem

Existing technologies make it difficult to prepare multi-layered nested carbon nanotubes, which limits their application potential in composite materials. Furthermore, existing methods have difficulty controlling the tube wall thickness and the size of the inter-tube cavities.

Method used

Multilayer nested carbon nanotubes were prepared using a template method. By combining MnO2 nanowires with dopamine and tetraethyl orthosilicate, and then removing SiO2 with heat treatment and an etchant, a multilayer CNT structure was formed, allowing control over the tube wall thickness and cavity size.

Benefits of technology

The controllable fabrication of multilayer CNTs has been achieved, improving thermal conductivity, electrical conductivity, and electromagnetic shielding performance, while also enhancing structural stability and strength, and expanding the application range of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117228660B_ABST
    Figure CN117228660B_ABST
Patent Text Reader

Abstract

The present invention relates to a multi-layer nested carbon nanotube and a preparation method thereof, a nanostructure formed by nesting multiple layers of CNT and a preparation method thereof. The multi-layer nested structure gives it higher thermal conductivity, electrical conductivity and electromagnetic shielding performance, improving the problem that the performance of ordinary single-layer CNT cannot reach the theoretical level due to its own defects. In addition, the multi-layer CNT also has higher structural stability and strength, and can also improve the fracture toughness of the material through the slippage between different CNT layers when facing an external load. The technical solution is simple, the process is controllable, the raw material cost is low, and it has broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to a method for preparing carbon nanotubes, and relates to a multi-layer nested carbon nanotube and a preparation method thereof, and particularly to a method for preparing multi-layer carbon nanotubes by a catalyst-free template method. Background Art

[0002] Carbon nanotubes (CNTs), as a typical representative of one-dimensional carbon nanomaterials, are seamless hollow tubular structures formed by curling single or multi-layer graphene sheets, in which each carbon atom is connected to three other adjacent carbon atoms in a sp 2 Hybridization is dominant, but sp 3 Hybridization situation. The defective structure in CNT causes its electrical and thermal conductivity to fail to reach the theoretical level. Therefore, in order to further develop the functions of CNT and give it higher mechanical, thermal, electrical and electromagnetic shielding properties, the researchers designed a new double-tube structure. The double-tube structure is composed of two layers of coaxial CNT nesting. Compared with the single-layer CNT, the double-tube structure is more stable, especially when the radius is large. The double-layer nested CNT structure is significantly better than the single-layer CNT in terms of stability and strength in the cross-sectional direction, and its conductivity is significantly improved. Reference 1 "Ye JC, Liu L, Oakdale1 J, et al. Ultra-low-density digitally architected carbon with astrutted tube-in-tube structure[J]. Nature Materials, 2021, 20: 1498-1505." The double-tube structure was prepared by a 3D printed polymer microlattice-nickel catalyzed two-step template pyrolysis process, and in an ultra-low density state (≤10 mg / cm 3 ), the double-layer CNT tube-in-tube structure is more than ten times harder than other carbon nanomaterials.

[0003] However, the preparation method mentioned in Document 1 uses the 3D printed template as the overall skeleton, and it is difficult to dope it into other components to modify the performance of the composite material, which limits the further application of the structure. In addition, the tube-in-tube structure prepared by nesting two layers of CNT has been proven to have better performance than a single-layer tube, but there is no relevant research on multi-layer CNT nested structures with more than two layers. The preparation method in Document 1 can only perform a single printing-nickel plating process, and ultimately only double-layer CNT can be obtained, which is not conducive to the development of multi-layer CNT structures.

[0004] Therefore, how to develop new technologies to achieve the nested structure of multi-layer CNTs without destroying the CNT structure is of great significance to further explore the application potential of CNTs. Summary of the invention

[0005] Technical issues to be solved

[0006] In order to avoid the shortcomings of the prior art, the present invention proposes a multi-layer nested carbon nanotube and a preparation method thereof, which is a method for preparing multi-layer nested CNTs using a template method, has a simple process and a wide range of preparation conditions, and the wall thickness of the prepared multi-layer CNTs and the size of the cavities between the tubes are controllable.

[0007] Technical Solution

[0008] A method for preparing multi-layer nested carbon nanotubes, comprising the following steps:

[0009] Step 1: Ultrasonic dispersion of MnO2 nanowires in Tris aqueous solution, then adding dopamine hydrochloride to the solution, stirring continuously for 12 to 24 hours, and then washing with deionized water to obtain MnO2@PDA composite nanowires;

[0010] Step 2: Ultrasonic dispersion of MnO2@PDA composite nanowires in anhydrous ethanol, adding deionized water and NH3·H2O, and then adding tetraethyl orthosilicate to the solution. After magnetic stirring for 2-6 h, MnO2@PDA@SiO2 composite nanowires were collected by multiple centrifugation.

[0011] Step 3: Place the MnO2@PDA@SiO2 composite nanowires in an oxalic acid solution and soak them in a 50~100 ºC water bath for 2~8 hours to remove the MnO2 nanowires and obtain PDA@SiO2 hollow tubes;

[0012] Step 4: Ultrasonic dispersion of the PDA@SiO2 hollow tubes in a Tris aqueous solution, then adding dopamine hydrochloride to the solution, stirring continuously for 12 to 24 hours, and then washing with deionized water to obtain PDA@SiO2@PDA composite nanowires;

[0013] Repeat steps 2 and 4 several times to obtain PDA@(SiO2@PDA) n Hollow tube;

[0014] Step 5: The obtained PDA@(SiO2@PDA) n The hollow tube was placed in a clean quartz crucible for carbonization, that is, placed in a tubular furnace with argon gas, heat treated at 600-1500 °C for 1-4 h with a gas flow rate of 50-500 sccm, and cooled to room temperature to obtain CNT@(SiO2@CNT) n Carbon nanotubes;

[0015] Step 6: CNT@(SiO2@CNT) nThe carbon nanotubes were placed in HF to react to remove SiO2, washed with deionized water several times and then dried in an oven at 60-100 °C to obtain multi-layer nested carbon nanotubes.

[0016] The preparation of the MnO2 nanowires is to mix MnSO4, KClO3 and CH3COOK, and dissolve them in deionized water in sequence; then add 2-10 mL of CH3COOH and transfer to a hydrothermal kettle, react in an oven at 120-200 ºC for 12-24 h, and wash, filter and dry the product to obtain MnO2 nanowires.

[0017] The molar ratio of MnSO4, KClO3 and CH3COOK is mixed at 1:1.5~2.5:1.2~2.0.

[0018] The 100-500 mg of MnO2 nanowires in step 1 correspond to 300-500 mL of a Tris aqueous solution with a concentration of 0.8-1.5 mg / mL and 100-500 mg of dopamine hydrochloride.

[0019] In the step 2, 100-500 mg of MnO2@PDA composite nanowires correspond to 300-500 mL of anhydrous ethanol, 50-150 mL of deionized water and 20-80 mL of NH3·H2O; and 1.0-5.0 g of tetraethyl orthosilicate.

[0020] The oxalic acid solution in step 3 is 0.5-1.0 mol / L.

[0021] In step 4, 100-500 mg of PDA@SiO2 corresponds to 300-500 mL of a Tris aqueous solution with a concentration of 0.8-1.5 mg / mL, and 100-500 mg of dopamine hydrochloride.

[0022] The carbon nanotube structure is multi-layer nesting, and the number of nesting layers is greater than or equal to two.

[0023] The wall thickness of each layer of the carbon nanotubes can be controlled by the process parameters of step 1 and step 4.

[0024] The size of the inter-tube cavities of each layer of the carbon nanotubes can be controlled by the process parameters of step 2.

[0025] Beneficial Effects

[0026] The present invention proposes a multi-layer nested carbon nanotube and a preparation method thereof, a nanostructure formed by nesting multiple layers of CNT and a preparation method thereof. The multi-layer nested structure gives it higher thermal conductivity, electrical conductivity and electromagnetic shielding performance, improving the problem that the performance of ordinary single-layer CNT cannot reach the theoretical level due to its own defects. In addition, the multi-layer CNT also has higher structural stability and strength, and can also improve the fracture toughness of the material through the slippage between different CNT layers when facing an external load. The technical solution is simple, the process is controllable, the raw material cost is low, and it has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 : Scanning electron micrograph of the double-layer CNT structure prepared in Example 1;

[0028] Figure 2 : Scanning electron micrograph of the three-layer CNT structure prepared in Example 2 DETAILED DESCRIPTION

[0029] The present invention will now be further described with reference to the embodiments and the accompanying drawings:

[0030] A method for preparing multi-layer nested carbon nanotubes, characterized in that the preparation method is as follows:

[0031] Step 1: Mix MnSO4, KClO3 and CH3COOK in a molar ratio of 1:1.5~2.5:1.2~2.0, and dissolve them in 60~100 mL of deionized water in turn; add 2~10 mL of CH3COOH to the solution; transfer to a hydrothermal autoclave, react in an oven at 120~200 ºC for 12~24 h, and wash, filter and dry the product to obtain MnO2 nanowires.

[0032] Step 2: Ultrasonic disperse 100~500 mg of MnO2 nanowire sample into 300~500 mL of Tris aqueous solution with a concentration of 0.8~1.5 mg / mL, then slowly add 100~500 mg of dopamine hydrochloride to the solution, stir continuously for 12~24 hours, and rinse with deionized water to obtain MnO2@PDA composite nanowires.

[0033] Step 3: Take 100-500 mg of MnO2@PDA composite nanowires, ultrasonically disperse them in 300-500 mL of anhydrous ethanol, add 50-150 mL of deionized water and 20-80 mL of NH3·H2O, then slowly add 1.0-5.0 g of tetraethyl orthosilicate to the solution, stir magnetically for 2-6 h, and collect the MnO2@PDA@SiO2 composite nanowires by multiple centrifugation.

[0034] Step 4: Place the prepared MnO2@PDA@SiO2 composite nanowires in a 0.5~1.0 mol / L oxalic acid solution and soak them in a 50~100 ºC water bath for 2~8 h to remove the MnO2 nanowires and obtain PDA@SiO2 hollow tubes.

[0035] Step 5: Ultrasonic disperse 100~500 mg of PDA@SiO2 hollow tubes into 300~500 mL of 0.8~1.5 mg / mL Tris aqueous solution, then slowly add 100~500 mg of dopamine hydrochloride to the solution. After continuous stirring for 12~24 hours, rinse with deionized water to obtain PDA@SiO2@PDA composite nanowires.

[0036] Repeat steps 3 and 5 to obtain PDA@(SiO2@PDA) n Composite nanowires.

[0037] Step 6: PDA@(SiO2@PDA) n The hollow tube was placed in a clean quartz crucible for carbonization, that is, the sample was placed in a tubular furnace with argon gas, heat treated at 600-1500 °C for 1-4 h, with a gas flow rate of 50-500 sccm, and cooled to room temperature to obtain CNT@(SiO2@CNT) n Self-supporting foam.

[0038] Step 7: CNT@(SiO2@CNT) n The foam was placed in HF to react to remove SiO2, washed with deionized water several times and then dried in an oven at 60-100 °C to obtain multi-layer nested carbon nanotubes.

[0039] Example 1:

[0040] Step 1: Weigh 0.676 g of MnSO4, 0.858 g of KClO3 and 0.588 g of CH3COOK, and dissolve them in 60 mL of deionized water in turn; add 4 mL of CH3COOH to the solution; transfer to a hydrothermal autoclave, react in an oven at 160 ºC for 12 h, wash, filter and dry the product to obtain MnO2 nanowires.

[0041] Step 2: Ultrasonic disperse 300 mg of MnO2 nanowire sample into 375 mL of 1.2 mg / mL Tris aqueous solution, then slowly add 300 mg of dopamine hydrochloride into the solution. After continuous stirring for 24 hours, rinse with deionized water to obtain MnO2@PDA composite nanowires.

[0042] Step 3: Take 300 mg of MnO2@PDA composite nanowires, ultrasonically disperse them in 300 mL of anhydrous ethanol, add 90 mL of deionized water and 30 mL of NH3·H2O, then slowly add 2.4 g of tetraethyl orthosilicate to the solution, stir magnetically for 4 h, and collect the MnO2@PDA@SiO2 composite nanowires after multiple centrifugation.

[0043] Step 4: Place the prepared MnO2@PDA@SiO2 composite nanowires in a 0.5 mol / L oxalic acid solution and soak them in a 70ºC water bath for 4 h to remove the MnO2 nanowires and obtain PDA@SiO2 hollow tubes.

[0044] Step 5: Ultrasonic disperse 300 mg of PDA@SiO2 composite nanowire sample into 375 mL of 1.2 mg / mL Tris aqueous solution, then slowly add 300 mg of dopamine hydrochloride into the solution. After continuous stirring for 24 hours, rinse with deionized water to obtain PDA@SiO2@PDA composite nanowires.

[0045] Step 6: Place the obtained PDA@SiO2@PDA hollow tube in a clean quartz crucible for carbonization, that is, place the sample in a tubular furnace filled with argon gas, heat treat it at 1050 °C for 2 h with a gas flow rate of 50 sccm, and obtain CNT@SiO2@CNT self-supporting foam after cooling to room temperature.

[0046] Step 7: Place the CNT@SiO2@CNT foam in HF to react to remove SiO2, wash it with deionized water several times, and then dry it in an oven at 60 °C to obtain Figure 1 Double-layer CNT self-supporting foam shown.

[0047] Example 2:

[0048] Step 1: Weigh 0.676 g of MnSO4, 0.979 g of KClO3 and 0.784 g of CH3COOK, and dissolve them in 80 mL of deionized water in turn; add 6 mL of CH3COOH to the solution; transfer to a hydrothermal autoclave, react in an oven at 180 ºC for 16 h, and wash, filter and dry the product to obtain MnO2 nanowires.

[0049] Step 2: Ultrasonic disperse 400 mg of MnO2 nanowire sample into 350 mL of 1.5 mg / mL Tris aqueous solution, then slowly add 400 mg of dopamine hydrochloride into the solution. After continuous stirring for 16 hours, rinse with deionized water to obtain MnO2@PDA composite nanowires.

[0050] Step 3: Take 400 mg of MnO2@PDA composite nanowires, ultrasonically disperse them in 400 mL of anhydrous ethanol, add 60 mL of deionized water and 50 mL of NH3·H2O, then slowly add 3.0 g of tetraethyl orthosilicate to the solution, stir magnetically for 6 h, and collect the MnO2@PDA@SiO2 composite nanowires after multiple centrifugation.

[0051] Step 4: Place the prepared MnO2@PDA@SiO2 composite nanowires in a 0.8 mol / L oxalic acid solution and soak them in an 80ºC water bath for 8 h to remove the MnO2 nanowires and obtain PDA@SiO2 hollow tubes.

[0052] Step 5: Ultrasonic disperse 400 mg of PDA@SiO2 composite nanowire sample into 350 mL of 1.5 mg / mL Tris aqueous solution, then slowly add 400 mg of dopamine hydrochloride into the solution. After continuous stirring for 16 hours, rinse with deionized water to obtain PDA@SiO2@PDA composite nanowires.

[0053] Step 6: Take 400 mg of PDA@SiO2@PDA nanowires, ultrasonically disperse them in 400 mL of anhydrous ethanol, continue to add 60 mL of deionized water and 50 mL of NH3·H2O, and then slowly add 3.0 g of tetraethyl orthosilicate to the solution. After magnetic stirring for 6 h, collect the PDA@SiO2@PDA@SiO2 composite nanowires after multiple centrifugation.

[0054] Step 7: Use ultrasound to ultrasonically disperse 400 mg of PDA@SiO2@PDA@SiO2 composite nanowire sample into 350 mL of 1.5 mg / mL Tris aqueous solution, then slowly add 400 mg of dopamine hydrochloride to the solution. After continuous stirring for 16 hours, rinse with deionized water to prepare PDA@(SiO2@PDA)2 composite nanowires.

[0055] Step 8: Place the obtained PDA@(SiO2@PDA)2 hollow tube in a clean quartz crucible for carbonization, that is, place the sample in a tubular furnace filled with argon gas, heat treat it at 1200 °C for 1 h with a gas flow rate of 200 sccm, and obtain CNT@(SiO2@CNT)2 self-supporting foam after cooling to room temperature.

[0056] Step 9: Place the CNT@(SiO2@CNT)2 foam in HF to react to remove SiO2, wash it with deionized water several times, and then dry it in an oven at 80 °C to obtain Figure 2 Three-layer CNT self-supporting foam shown.

[0057] By changing the process parameters of step 2 and step 5, the wall thickness of each layer of the carbon nanotubes can be controlled.

[0058] Through the process parameters of step 3, the size of the inter-tube cavity of each layer of the carbon nanotubes can be controlled.

[0059] Example 3:

[0060] Step 1: Weigh 0.676 g of MnSO4, 0.858 g of KClO3 and 0.588 g of CH3COOK, dissolve them in 100 mL of deionized water in turn; add 6 mL of CH3COOH to the solution; transfer to a hydrothermal autoclave, react in an oven at 150 ºC for 12 h, wash, filter and dry the product to obtain MnO2 nanowires.

[0061] Step 2: Ultrasonic disperse 200 mg of MnO2 nanowire sample into 375 mL of 1.0 mg / mL Tris aqueous solution, then slowly add 200 mg of dopamine hydrochloride into the solution. After continuous stirring for 18 hours, rinse with deionized water to obtain MnO2@PDA composite nanowires.

[0062] Step 3: Take 400 mg of MnO2@PDA composite nanowires, ultrasonically disperse them in 400 mL of anhydrous ethanol, add 100 mL of deionized water and 60 mL of NH3·H2O, and then slowly add 4.0 g of tetraethyl orthosilicate to the solution. After magnetic stirring for 6 h, the MnO2@PDA@SiO2 composite nanowires were collected by multiple centrifugation.

[0063] Step 4: Place the prepared MnO2@PDA@SiO2 composite nanowires in a 0.5 mol / L oxalic acid solution and soak them in a 60ºC water bath for 8 h to remove the MnO2 nanowires and obtain PDA@SiO2 hollow tubes.

[0064] Step 5: Ultrasonic disperse 200 mg of PDA@SiO2 composite nanowire sample into 375 mL of 1.0 mg / mL Tris aqueous solution, then slowly add 200 mg of dopamine hydrochloride into the solution. After continuous stirring for 18 hours, rinse with deionized water to obtain PDA@SiO2@PDA composite nanowires.

[0065] Step 6: The obtained PDA@SiO2@PDA hollow tube was placed in a clean quartz crucible for carbonization, that is, the sample was placed in a tubular furnace filled with argon gas, heat treated at 900 °C for 2 h with a gas flow rate of 200 sccm, and after cooling to room temperature, CNT@SiO2@CNT self-supporting foam was obtained.

[0066] Step 7: Place the CNT@SiO2@CNT foam in HF to react to remove SiO2, wash it with deionized water several times and then dry it in an oven at 70 °C to obtain a double-layer CNT self-supporting foam.

[0067] The technical solution of the present invention is not limited to the specific implementation methods listed above, and various changes can be made. That is, all other embodiments obtained according to the claims and description of the present invention application belong to the protection scope of the present invention.

Claims

1. A method for preparing multi-layer nested carbon nanotubes, characterized in that Here are the steps: Step 1: Ultrasonic dispersion of MnO2 nanowires in Tris aqueous solution, then adding dopamine hydrochloride to the solution, stirring continuously for 12 to 24 hours, and then washing with deionized water to obtain MnO2@PDA composite nanowires; Step 2: ultrasonically disperse the MnO2@PDA composite nanowires in anhydrous ethanol, add deionized water and NH3·H2O, then add tetraethyl orthosilicate to the solution, stir magnetically for 2-6 h, and then collect the MnO2@PDA@SiO2 composite nanowires by multiple centrifugation; Step 3: Place the MnO2@PDA@SiO2 composite nanowires in an oxalic acid solution and soak them in a 50-100 ºC water bath for 2-8 h to remove the MnO2 nanowires and obtain PDA@SiO2 hollow tubes; Step 4: Ultrasonic dispersion of the PDA@SiO2 hollow tubes in a Tris aqueous solution, then adding dopamine hydrochloride to the solution, stirring continuously for 12 to 24 hours, and then washing with deionized water to obtain PDA@SiO2@PDA composite nanowires; Repeat steps 2 and 4 several times to obtain PDA@(SiO2@PDA) n Hollow tube; Step 5: The obtained PDA@(SiO2@PDA) n The hollow tube was placed in a clean quartz crucible for carbonization, that is, placed in a tubular furnace with argon gas, heat treated at 600-1500 °C for 1-4 h with a gas flow rate of 50-500 sccm, and cooled to room temperature to obtain CNT@(SiO2@CNT) n Carbon nanotubes; Step 6: CNT@(SiO2@CNT) n The carbon nanotubes were placed in HF to react and remove SiO2, and then washed with deionized water for several times and dried in an oven at 60-100 °C to obtain multi-layer nested carbon nanotubes. The preparation of the MnO2 nanowires is as follows: MnSO4, KClO3 and CH3COOK are mixed and dissolved in deionized water in sequence; 2-10 mL of CH3COOH is then added dropwise and transferred to a hydrothermal reactor, reacted in an oven at 120-200 ºC for 12-24 h, and the product is washed, filtered and dried to obtain the MnO2 nanowires; The 100-500 mg of MnO2 nanowires in step 1 correspond to 300-500 mL of a Tris aqueous solution with a concentration of 0.8-1.5 mg / mL and 100-500 mg of dopamine hydrochloride.

2. The method for preparing multi-layer nested carbon nanotubes according to claim 1, characterized in that: The molar ratio of MnSO4, KClO3 and CH3COOK is mixed at 1:1.5~2.5:1.2~2.

0.

3. The method for preparing multi-layer nested carbon nanotubes according to claim 1, characterized in that: In the step 2, 100-500 mg of MnO2@PDA composite nanowires correspond to 300-500 mL of anhydrous ethanol, 50-150 mL of deionized water, and 20-80 mL of NH3·H2O; and 1.0-5.0 g of tetraethyl orthosilicate.

4. The method for preparing multi-layer nested carbon nanotubes according to claim 1, characterized in that: The oxalic acid solution in step 3 is 0.5-1.0 mol / L.

5. The method for preparing multi-layer nested carbon nanotubes according to claim 1, characterized in that: In step 4, 100-500 mg of PDA@SiO2 corresponds to 300-500 mL of a Tris aqueous solution with a concentration of 0.8-1.5 mg / mL, and 100-500 mg of dopamine hydrochloride.

6. The method for preparing multi-layer nested carbon nanotubes according to claim 1, characterized in that: The wall thickness of each layer of the carbon nanotubes can be controlled by the process parameters of step 1 and step 4.

7. The method for preparing multi-layer nested carbon nanotubes according to claim 1, characterized in that: The size of the inter-tube cavities of each layer of the carbon nanotubes can be controlled by the process parameters of step 2.

8. A multi-layered nested carbon nanotube prepared by the method according to any one of claims 1 to 7, characterized in that: The carbon nanotube structure is multi-layer nesting, and the number of nesting layers is greater than or equal to two.