A new soil admixture for solidifying slag into ecological roadbed, preparation method and use thereof
By combining raw materials such as manganese sulfate or acrylic acid with desulfurization gypsum, ferrous sulfate, etc., a multi-core complex was formed, which solved the problem of low compressive strength of existing soil curing admixtures, and achieved high compressive strength and stability of the slag meets the requirements of the grassroots roads.
Patent Information
- Application Number
- CN202311098783.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-29
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-08-29
AI Technical Summary
The existing new soil curing admixtures have poor stability and low compressive strength, which cannot meet the high-strength needs of road bases.
Using raw materials such as manganese sulfate or acrylic acid, desulfurization gypsum, ferrous sulfate, sodium silicate, sodium fluorosilicate, cement, fly ash and seawater slag in power plant, a new soil is formed by stirring and heating reaction. and triethanolamine is added at room temperature and heating conditions to form a multi-nuclear complex to improve the stability and compressive strength of the slag.
The high compressive strength of the slag was achieved, and the 7-day unlimited compressive strength reached 0.96~1.33Mpa, which met the compressive strength requirements of the road cushion base layer, surface base layer and stable layer, significantly improving the stability and strength of the slag. .
Smart Images

Figure CN117229016B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a soil admixture for solidifying slag into an ecological roadbed, in particular to a novel soil admixture for solidifying slag into an ecological roadbed, a preparation method and application thereof. Background Art
[0002] The stacking of slag-soil mixture not only occupies a large amount of land resources, but also causes soil erosion, pollution and various safety hazards. Power plant seawater slag is ash slag produced by some thermal power plants during the energy conversion process. The slag flushing water is seawater, and the ash slag produced becomes seawater slag. At present, soil remediation and protection are mainly carried out through new soil solidification admixtures. New soil solidification admixtures are added to the soil to improve the engineering properties of the soil through physical and (or) chemical reactions with inorganic binders, soil and water.
[0003] However, the existing new soil solidification admixtures have poor stability and low compressive strength, only 0.4 to 0.6 MPa. Summary of the invention
[0004] In order to solve the above problems, the present invention provides a soil admixture with high compressive strength and good stability for solidifying slag into an ecological roadbed. The specific technical solution is as follows:
[0005] A soil admixture for solidifying slag into an ecological roadbed is prepared from the following raw materials in parts by mass: 36-43 parts of manganese sulfate or acrylic acid, or a mixture of the two; 10-15 parts of desulfurized gypsum; 3-5 parts of ferrous sulfate; 4-8 parts of triethanolamine; 3-5 parts of sodium silicate; 2-6 parts of sodium fluorosilicate; 13-23 parts of silicate cement; 5-10 parts of fly ash; and 3-5 parts of seawater slag from a power plant.
[0006] A method for preparing a soil admixture for solidifying slag into an ecological roadbed, used for the above-mentioned soil admixture for solidifying slag into an ecological roadbed, characterized in that it comprises the following steps:
[0007] Aluminum sulfate, desulfurized gypsum, ferrous sulfate, sodium fluorosilicate, silicate cement, fly ash, and seawater slag from a power plant are placed in a reaction kettle;
[0008] Add manganese sulfate or acrylic acid, and sodium silicate while stirring;
[0009] Stir at room temperature for 0.2 to 1.5 hours;
[0010] Heat to 80-95°C and stir for 0.5-1.5h;
[0011] Stop heating and cool to 75-85°C, add triethanolamine;
[0012] Stir at a constant temperature of 78-82°C for 0.2-1h;
[0013] The mixture is rapidly cooled to 35-45° C., discharged and filtered to obtain the soil admixture for solidifying the slag into an ecological roadbed.
[0014] A use of a soil admixture for solidifying slag into an ecological roadbed, which is used for a cushion base, a surface base, and a stabilizing layer.
[0015] Preferably, the cushion base comprises: 2% of the soil admixture for solidifying slag into an ecological roadbed; 0.5% of PO42.5 cement; and the remainder is a slag-soil mixture.
[0016] Preferably, the surface base layer comprises: 3% of the soil admixture for solidifying slag into an ecological roadbed; 1% of PO42.5 cement; and the remainder is a slag-soil mixture.
[0017] Preferably, the stabilization layer comprises: 5% of the soil admixture for solidifying slag into an ecological roadbed; 3% of PO42.5 cement; and the remainder is a slag-soil mixture.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] The invention provides a novel soil admixture for solidifying slag into an ecological roadbed, which has high compressive strength and good stability.
[0020] The above-mentioned embodiments of the present application have been tested by the Highway Engineering Testing Center of the Ministry of Transport in accordance with GB / T50266-2013, and the 7-day unconfined compressive strength (saturated with water) reaches 0.96~1.33Mpa, which meets the compressive strength requirements of the cushion base, surface base and stabilization layer of various types of roads.
[0021] The seawater slag from power plants contains a large amount of chloride ions, sulfate ions, calcium oxide, magnesium oxide, etc. The present application forms crystals with sodium fluorosilicate and calcium ions, magnesium ions, etc. in the materials and slag soil to increase the strength and density of the soil, thereby greatly improving the stability and strength of the slag soil.
[0022] Aluminum sulfate, manganese sulfate, ferrous sulfate, etc. are added in the present application. Ferrous sulfate has a relatively strong reducing property and can reduce chromate in the slag soil. Triethanolamine reacts with metal ions such as aluminum ions, manganese ions, magnesium ions, iron ions, etc. to form a multi-nuclear complex in the slag soil, so that the structural layer has a greater bearing capacity and compressive strength.
[0023] At the same time, triethanolamine is beneficial to improving the fixation capacity of chloride ions, promoting hydration in slag soil, promoting physical bonding, increasing the density of slag soil, and greatly improving the stability and strength of slag soil. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1It is a comparison diagram of the present invention and the prior art. DETAILED DESCRIPTION
[0025] The present invention will be further described with reference to the accompanying drawings.
[0026] Embodiment 1
[0027] For padding:
[0028] 3-8 parts by mass of aluminum sulfate, 10-15 parts by mass of desulfurized gypsum, 3-5 parts by mass of ferrous sulfate, 2-6 parts by mass of sodium fluorosilicate, 13-23 parts by mass of Portland cement, 5-10 parts by mass of fly ash, and 3-5 parts by mass of seawater slag from a power plant are put into a reactor and stirred at a stirring speed of 100 r / min;
[0029] Add 36-43 parts by mass of manganese sulfate and 3-5 parts by mass of sodium silicate, and stir the above raw materials thoroughly at room temperature;
[0030] The mixture was stirred at room temperature for 0.2 h, then heated to a temperature of about 80-95°C, and then kept warm and stirred for 1 h; immediately the heating was stopped to cool the mixture down. When the temperature of the material dropped to about 75-85°C, 4-8 parts by weight of triethanolamine was added, and the mixture was stirred at a constant temperature of about 78-82°C for 0.5 h, and then the heating was stopped to rapidly reduce the temperature. When the mixture was cooled to about 34-45°C, the material was filtered to obtain a soil admixture for solidifying slag into an ecological roadbed.
[0031] A soil admixture for solidifying slag into an ecological roadbed has a fineness of 80 μm and a square hole sieve residue of no more than 15%.
[0032] Slag soil mixture: a large amount of construction waste slag, sludge, power plant seawater slag, mine tailings, seawater slag, fly ash non-hazardous mud and various industrial solid wastes
[0033] A soil admixture for solidifying slag into an ecological roadbed is configured according to the following table:
[0034] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Aluminum sulfate 3 4 5 6 7 8 Manganese sulfate 36 37 38 40 42 43 Desulfurization gypsum 15 14 13 12 11 10 Ferrous Sulfate 3 5 4.5 3.5 4 3.5 Triethanolamine 4 8 5 7 6 5.5 Sodium silicate 3 4.5 3.5 4 5 3.5 Sodium Fluorosilicate 2 5 6 4 3.5 3 Portland cement 13 20 23 19 14 16 Fly ash 5 8 6 10 9 7 Power plant seawater slag 3 4 5 4.5 3.5 4
[0035] The cushion base comprises 2% of the soil admixture for solidifying the slag into an ecological roadbed; 0.5% of PO42.5 cement; and the remainder is a slag-soil mixture.
[0036] Unconfined compressive strength test record of the above-mentioned cushion base:
[0037]
[0038] Obviously, when used for cushion base, the compressive strength is 0.96~1.31Mpa, which can meet the requirements of cushion base.
[0039] Embodiment 2
[0040] For surface base:
[0041] 3-8 parts by mass of aluminum sulfate, 10-15 parts by mass of desulfurized gypsum, 3-5 parts by mass of ferrous sulfate, 2-6 parts by mass of sodium fluorosilicate, 13-23 parts by mass of Portland cement, 5-10 parts by mass of fly ash, and 3-5 parts by mass of seawater slag from a power plant are put into a reactor and stirred at a stirring speed of 100 r / min;
[0042] Add 36-43 parts by weight of a mixture of manganese sulfate and acrylic acid and 3-5 parts by weight of sodium silicate, and stir the above raw materials thoroughly at room temperature;
[0043] The mixture was stirred at room temperature for 0.2 h, then heated to a temperature of about 80-95°C, and then kept warm and stirred for 1 h; immediately the heating was stopped to cool the mixture down. When the temperature of the material dropped to about 75-85°C, 4-8 parts by weight of triethanolamine was added, and the mixture was stirred at a constant temperature of about 78-82°C for 0.5 h, and then the heating was stopped to rapidly reduce the temperature. When the mixture was cooled to about 34-45°C, the material was filtered to obtain a soil admixture for solidifying slag into an ecological roadbed.
[0044] When used for the surface base layer, a mixture of manganese sulfate and acrylic acid is used, with the content of both being 20-80%.
[0045] A soil admixture for solidifying slag into an ecological roadbed has a fineness of 80 μm and a square hole sieve residue of no more than 15%.
[0046] A soil admixture for solidifying slag into an ecological roadbed is configured according to the following table:
[0047] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Aluminum sulfate 8 3 5 5 6 8 Manganese sulfate and acrylic acid mixture 38 35 36 43 41 40 Desulfurization gypsum 10 13 12.5 14.5 14 15 Ferrous Sulfate 3.5 4.5 4 3 4 3.5 Triethanolamine 8 7 7 4 5 5.5 Sodium silicate 5 4 5 4.5 4 3.5 Sodium Fluorosilicate 2.5 6 4 5 3 3.5 Portland cement 22 13 20 17 19 15 Fly ash 7 6.5 7.5 5 7 10 Power plant seawater slag 5 3 4 3.5 4 3.5
[0048] The surface base comprises: 3% of a soil admixture for solidifying slag soil into an ecological roadbed; 1% of PO42.5 cement; and the remaining material is a slag soil mixture.
[0049] Unconfined compressive strength test record of the above surface base:
[0050]
[0051] Obviously, when used for surface base, the compressive strength is 1.21~1.33Mpa, which can meet the requirements of surface base.
[0052] Embodiment 3
[0053] For stabilization layer:
[0054] 3-8 parts by mass of aluminum sulfate, 10-15 parts by mass of desulfurized gypsum, 3-5 parts by mass of ferrous sulfate, 2-6 parts by mass of sodium fluorosilicate, 13-23 parts by mass of Portland cement, 5-10 parts by mass of fly ash, and 3-5 parts by mass of seawater slag from a power plant are put into a reactor and stirred at a stirring speed of 100 r / min;
[0055] Add 36-43 parts by weight of a mixture of manganese sulfate and acrylic acid and 3-5 parts by weight of sodium silicate, and stir the above raw materials thoroughly at room temperature;
[0056] The mixture was stirred at room temperature for 0.2 h, then heated to a temperature of about 80-95°C, and then kept warm and stirred for 1 h; immediately the heating was stopped to cool the mixture down. When the temperature of the material dropped to about 75-85°C, 4-8 parts by weight of triethanolamine was added, and the mixture was stirred at a constant temperature of about 78-82°C for 0.5 h, and then the heating was stopped to rapidly reduce the temperature. When the mixture was cooled to about 34-45°C, the material was filtered to obtain a soil admixture for solidifying slag into an ecological roadbed.
[0057] When used for the stabilizing layer, a mixture of manganese sulfate and acrylic acid is used, with the content of both being 20-80%.
[0058] A soil admixture for solidifying slag into an ecological roadbed has a fineness of 80 μm and a square hole sieve residue of no more than 15%.
[0059] A soil admixture for solidifying slag into an ecological roadbed is configured according to the following table for the stabilization layer:
[0060] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Aluminum sulfate 3.5 5.5 4 5.5 7.5 7 Manganese sulfate and acrylic acid mixture 40 36 42 41 39 38 Desulfurization gypsum 10.5 12 15 10 14 11.5 Ferrous Sulfate 3.5 4 5 4.5 5 4 Triethanolamine 8 7 7 5 7 6 Sodium silicate 5 4.5 3 4.5 3.5 5 Sodium Fluorosilicate 6 6 5.5 3.5 4 3 Portland cement 15 18 20 21 13 19 Fly ash 8 5 6 6.5 5 9 Power plant seawater slag 3.5 3 4.5 5 3 4.5
[0061] The stabilization layer includes: 3% of a soil admixture for solidifying the slag into an ecological roadbed; 1% of PO42.5 cement; and the rest is a slag-soil mixture.
[0062] Unconfined compressive strength test record of the above stabilization layer:
[0063]
[0064] Obviously, when used for the base layer, the compressive strength is 1.19~1.33Mpa, which can meet the requirements of the stabilization layer.
[0065] The above-mentioned embodiments of the present application have been tested by the Highway Engineering Testing Center of the Ministry of Transport in accordance with GB / T50266-2013, and the 7-day unconfined compressive strength (saturated with water) reaches 0.96 to 1.33 MPa, meeting the strength requirements of the base and subbase of various types of roads.
[0066] like Figure 1As shown, part 1 is the soil admixture used in the present application to solidify the debris into an ecological roadbed, and part 2 is the addition of the existing admixture. Obviously, the indentation of part 2 is deeper than that of part 1, that is, the compressive strength of part 2 is not as high as the compressive strength of the soil admixture used in the present application to solidify the debris into an ecological roadbed.
[0067] Comparative Example 1
[0068] No power plant seawater slag is added.
[0069] 3 parts by mass of aluminum sulfate, 10 parts by mass of desulfurized gypsum, 3 parts by mass of ferrous sulfate, 2 parts by mass of sodium fluorosilicate, 13 parts by mass of Portland cement, and 5 parts by mass of fly ash were added into a reactor and stirred at a stirring speed of 100 r / min;
[0070] Add 36 parts by mass of manganese sulfate and 3 parts by mass of sodium silicate, and stir the above raw materials thoroughly at room temperature;
[0071] The mixture was stirred at room temperature for 0.2 h, then heated to about 80°C, and then kept warm and stirred for 1 h. The heating was then stopped to cool the mixture. When the temperature of the material dropped to about 75°C, 6 parts by weight of triethanolamine was added. The mixture was stirred at a constant temperature of about 78°C for 0.5 h, and then the heating was stopped to rapidly reduce the temperature. When the mixture was cooled to about 34°C, the material was filtered to obtain a soil admixture for solidifying slag into an ecological roadbed.
[0072] A soil admixture for solidifying slag into an ecological roadbed has a fineness of 80 μm and a square hole sieve residue of no more than 15%.
[0073] The cushion base comprises 2% of the soil admixture for solidifying the slag into an ecological roadbed; 0.5% of PO42.5 cement; and the remainder is a slag-soil mixture.
[0074] The tested compressive strength is 0.53Mpa, which is significantly less than 1.33Mpa.
[0075] The absence of seawater slag from power plants reduces chloride ions, sulfate ions, calcium oxide and magnesium oxide, resulting in fewer crystals formed by sodium fluorosilicate and calcium ions, magnesium ions and other ions in materials and slag soil, reducing the stability and strength of the slag soil.
[0076] Comparative Example 2
[0077] No triethanolamine was added.
[0078] 4 parts by mass of aluminum sulfate, 11 parts by mass of desulfurized gypsum, 3.5 parts by mass of ferrous sulfate, 3 parts by mass of sodium fluorosilicate, 14 parts by mass of Portland cement, 6 parts by mass of fly ash, and 3.5 parts by mass of seawater slag from a power plant were added into a reactor and stirred at a stirring speed of 100 r / min;
[0079] Add 37 parts by mass of a mixture of manganese sulfate and acrylic acid and 3.5 parts by mass of sodium silicate, and stir the above raw materials thoroughly at room temperature;
[0080] Stir at room temperature for 0.5h, then heat to about 85℃, and then keep stirring for 1h; then stop heating and cool it down. When the temperature of the material drops to about 80℃, let the temperature drop rapidly. When it cools to about 37℃, filter the material to obtain a soil admixture for solidifying slag into an ecological roadbed.
[0081] In this embodiment, the content of manganese sulfate is 20% by weight of the mixture, and the content of acrylic acid is 80% by weight of the mixture.
[0082] A soil admixture for solidifying slag into an ecological roadbed has a fineness of 80 μm and a square hole sieve residue of no more than 15%.
[0083] The surface base comprises: 3% of a soil admixture for solidifying slag soil into an ecological roadbed; 1% of PO42.5 cement; and the remaining material is a slag soil mixture.
[0084] The tested compressive strength is 0.48Mpa, which is significantly less than 1.33Mpa. The slag cannot form multi-nuclear complexes, which reduces the bearing capacity and compressive strength.
[0085] Comparative Example 3
[0086] No ferrous sulfate was added.
[0087] 4.5 parts by mass of aluminum sulfate, 12 parts by mass of desulfurized gypsum, 3.5 parts by mass of sodium fluorosilicate, 15 parts by mass of Portland cement, 6.5 parts by mass of fly ash, and 3.5 parts by mass of seawater slag from a power plant were added into a reactor and stirred at a stirring speed of 100 r / min.
[0088] Add 38 parts by weight of a mixture of manganese sulfate and acrylic acid and 3.5 parts by weight of sodium silicate, and stir the raw materials thoroughly at room temperature;
[0089] The mixture was stirred at room temperature for 0.5 h, then heated to a temperature of about 85°C, and then kept warm and stirred for 1 h; immediately the heating was stopped to cool the mixture down. When the temperature of the material dropped to about 80°C, 5 parts by weight of triethanolamine was added, and the mixture was stirred at a constant temperature of about 79°C for 0.5 h, and then the heating was stopped to rapidly reduce the temperature. When the mixture was cooled to about 37°C, the material was filtered to obtain a soil admixture for solidifying slag into an ecological roadbed.
[0090] In this embodiment, the content of manganese sulfate is 25% of the mass of the mixture of the two, and the content of acrylic acid is 75% of the mass of the mixture of the two.
[0091] A soil admixture for solidifying slag into an ecological roadbed has a fineness of 80 μm and a square hole sieve residue of no more than 15%.
[0092] The stabilization layer includes: 3% of a soil admixture for solidifying the slag into an ecological roadbed; 1% of PO42.5 cement; and the rest is a slag-soil mixture.
[0093] The tested compressive strength is 0.46Mpa, which is significantly less than 1.33Mpa. Due to the reduction of ferrous sulfate, the number of multi-nuclear complexes in the slag is reduced, which reduces the bearing capacity and compressive strength.
[0094] The technical principle of the present invention is described above in conjunction with specific embodiments. These descriptions are only for explaining the principle of the present invention and cannot be interpreted as limiting the protection scope of the present invention in any way. Based on the explanations herein, those skilled in the art can associate other specific implementations of the present invention without paying creative labor, and these methods will fall within the protection scope of the claims of the present invention.
Claims
1. A soil admixture for solidifying slag into an ecological roadbed, characterized in that: Made from the following raw materials in parts by mass: 3-8 parts of aluminum sulfate; 36-43 parts of manganese sulfate and / or acrylic acid; 10-15 parts of desulfurized gypsum; 3-5 parts of ferrous sulfate; 4 to 8 parts of triethanolamine; 3-5 parts of sodium silicate; 2-6 parts of sodium fluorosilicate; 13-23 parts of Portland cement; 5-10 parts of fly ash; 3-5 parts of seawater slag from power plants; The soil admixture for solidifying slag into an ecological roadbed is prepared by the following steps: Aluminum sulfate, desulfurized gypsum, ferrous sulfate, sodium fluorosilicate, silicate cement, fly ash, and seawater slag from a power plant are placed in a reaction kettle; Add manganese sulfate and / or acrylic acid, and sodium silicate while stirring; Stir at room temperature for 0.2 to 1.5 hours; Heat to 80-95°C and stir for 0.5-1.5h; Stop heating and cool to 75-85°C, add triethanolamine; Stir at a constant temperature of 78-82°C for 0.2-1h; The mixture is rapidly cooled to 35-45° C., discharged and filtered to obtain the soil admixture for solidifying the slag into an ecological roadbed.
2. The use of a soil admixture for solidifying slag into an ecological roadbed according to claim 1, characterized in that: Used for cushion base, surface base and stabilization layer.
3. The use of a soil admixture for solidifying slag into an ecological roadbed according to claim 2, characterized in that: The base layer comprises: 2% of the soil admixture for solidifying slag into an ecological roadbed; PO42.5 cement 0.5%; The remaining material is a mixture of slag and soil.
4. The use of a soil admixture for solidifying slag into an ecological roadbed according to claim 2, characterized in that: The surface base layer comprises: 3% of the soil admixture for solidifying the slag into an ecological roadbed; PO42.5 cement 1%; The remaining material is a mixture of slag and soil.
5. The use of a soil admixture for solidifying slag into an ecological roadbed according to claim 2, characterized in that: The stabilization layer comprises: 5% of the soil admixture for solidifying the slag into an ecological roadbed; PO42.5 cement 3%; The remaining material is a mixture of slag and soil.