A PBAT / PPCP polymer film and its preparation method and application in the field of biodegradable mulch film
By mixing PBAT and PPCP materials and introducing p-phenylenediamine as a compatibilizer, a new polymer with high barrier properties and mechanical strength is solved, and the problems of durability and degradation difficulty of agricultural mulch materials are achieved, achieving longer functions and higher agricultural output.
Patent Information
- Application Number
- CN202311449965.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-02
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-11-02
AI Technical Summary
The existing agricultural plastic film materials have poor durability, low strength and difficulty in degradation, resulting in soil pollution and ecological environment hazards. The single material has defects in barrier properties, mechanical strength and film forming processability.
The two materials PBAT and PPCP were mixed, and p-phenylenediamine was introduced as a compatible agent to pass through amine ester exchange reaction to form a new polymer with strong barrier properties and good mechanical strength. It was prepared through a twin-screw extruder and a film blowing mechanism. Made a polymer film.
It improves the compatibility and performance of the new polymer, extends the functional period of the mulch, improves mechanical properties and water vapor barrier properties, and promotes crop growth and agricultural benefits.
Smart Images

Figure CN117229612B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of polymer mulch films, and in particular, to a PBAT / PPCP polymer film and a preparation method thereof and application in the field of biodegradable mulch films. Background Art
[0002] Agricultural mulch is a mature cultivation technology in the agricultural planting process. It can maintain soil moisture, improve water utilization, alleviate soil water shortage in arid and semi-arid areas, and improve the growth environment of crops, which is conducive to crop growth and development, increase crop yields and agricultural benefits, ensure the increase of crop yields, and increase agricultural production benefits. However, once the seeds germinate and emerge during seedling cultivation, the mulch must be removed in time, otherwise, it is easy to burn the seedlings with high temperature; and after the crops are mature and harvested, the agricultural film loses its function, and the problem of agricultural film waste pollution follows. Due to the one-time use of mulch, a large amount of residual film is left in the soil every year.
[0003] Nowadays, agricultural mulch films made of chemicals such as polyethylene and polypropylene are commonly used on the market. In addition to their functions of heat preservation and weed control, they also have problems such as poor durability, low strength, and difficulty and long time to degrade. Because they are difficult to degrade and cannot be recycled for secondary use, a large amount of mulch film fragments will remain in the soil, which will not only destroy the soil structure, affect crop growth and lead to reduced production, but also cause serious environmental pollution. These mulch film fragments can form a barrier layer in the soil, which hinders the flow of water, air, fertilizer, etc. in the soil, causing the soil structure to become compacted, seriously endangering the ecological environment, and causing white pollution.
[0004] PBAT (polybutylene adipate / terephthalate) and PPCP (polypropylene copolymer) are currently the key alternative materials to solve the problem of plastic pollution. They have partially replaced traditional plastics in the fields of film materials and disposable plastic products. However, each material has its own defects, resulting in many defects in barrier properties, mechanical strength, film processing, etc. Summary of the invention
[0005] The purpose of the present application is to provide a PBAT / PPCP polymer film, which mixes PBAT and PPCP to form a new polymer with the advantages of strong barrier properties and good mechanical strength.
[0006] Another object of the present application is to provide a method for preparing a PBAT / PPCP polymer film, which is simple and convenient.
[0007] In order to solve the above technical problems, the technical solution adopted in this application is:
[0008] On the one hand, the present application provides a PBAT / PPCP polymer film, wherein the PBAT / PPCP polymer film comprises the following raw materials in weight percentage: 65-75% PBAT, 20-30% PPCP and 1-5% compatibilizer.
[0009] On the other hand, the present application provides a method for preparing a PBAT / PPCP polymer film, comprising the following steps:
[0010] S1, weighing each raw material, placing the raw material in a twin-screw extruder for granulation, and obtaining mixed granules;
[0011] S2. Blowing the mixed particles through a film blowing machine to obtain a polymer film.
[0012] An application of the above PBAT / PPCP polymer film in the field of biodegradable mulch films.
[0013] Compared with the prior art, the embodiments of the present application have at least the following advantages or beneficial effects:
[0014] Based on the characteristics that both PBAT and PPCP, two degradable polyester materials, contain ester groups, the present application introduces p-phenylenediamine as a compatibilizer, and realizes segment embedding between PBAT and PPCP through amine ester exchange reaction (amine ester exchange reaction occurs in ester compounds and can exchange hydroxyl groups therein, wherein the hydroxyl groups of ester reactants are replaced by amino groups of amine reactants to form compounds with amide bonds), thereby improving the compatibility between the two, and finally forming a new polymer that is stable and retains the advantages of both. After the new polymer is prepared into a degradable mulch film, it has comprehensive improvements in terms of blow molding film, mechanical properties, water vapor barrier properties and functional period compared with the original single material. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0016] Figure 1 This is a schematic diagram of the amine transesterification reaction of this application;
[0017] Figure 2 A physical picture of the sample prepared in Example 1 of the present application;
[0018] Figure 3 This is the infrared spectrum of the raw material PPCP of Example 1 of the present application;
[0019] Figure 4This is the infrared spectrum of the raw material PBAT of Example 1 of the present application;
[0020] Figure 5 The infrared spectrum of the sample prepared in Example 1 of the present application;
[0021] Figure 6 This is the melting curve diagram of the raw materials PPCP, PBAT and product 1 of Example 1 of the present application;
[0022] Figure 7 This is a crystallization curve diagram of the raw materials PPCP, PBAT and product 1 of Example 1 of the present application. DETAILED DESCRIPTION
[0023] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0024] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below with reference to specific embodiments.
[0025] A PBAT / PPCP polymer film comprises the following raw materials in weight percentage: 65-75% PBAT, 20-30% PPCP and 1-5% compatibilizer.
[0026] Amine transesterification occurs in ester compounds and can exchange hydroxyl groups therein, wherein the hydroxyl groups of the ester reactants are replaced by the amino groups of the amine reactants to form compounds with amide bonds. Figure 1 As shown. Based on the characteristics that both PBAT and PPCP degradable polyester materials contain ester groups, this application introduces p-phenylenediamine as a compatibilizer, realizes segment embedding between PBAT and PPCP through amine ester exchange reaction, thereby improving the compatibility between the two, and finally forms a stable new polymer that retains the advantages of both. After the new polymer is prepared into a degradable ground film, it has comprehensive improvements in blow molding film, mechanical properties, water vapor barrier properties and functional period compared with the original single material.
[0027] In some embodiments of the present application, the raw materials of the above PBAT / PPCP polymer film also include 1-5% masterbatch. The masterbatch can be used to adjust the color of the polymer film and broaden the application range of the product.
[0028] In some embodiments of the present application, the compatibilizer is p-phenylenediamine.
[0029] A method for preparing a PBAT / PPCP polymer film comprises the following steps:
[0030] S1, weighing each raw material, placing the raw material in a twin-screw extruder for granulation, and obtaining mixed granules;
[0031] S2. Blowing the mixed particles through a film blowing machine to obtain a polymer film.
[0032] In some embodiments of the present application, the granulation temperature in the above step S1 is 125-160°C.
[0033] In some embodiments of the present application, the blow molding temperature in the above step S1 is 150-175°C.
[0034] In some embodiments of the present application, the thickness of the polymer film is 8-15 μm.
[0035] An application of the above PBAT / PPCP polymer film in the field of biodegradable mulch films.
[0036] The features and performance of the present application are further described in detail below in conjunction with the embodiments.
[0037] Example 1
[0038] A PBAT / PPCP polymer film comprises the following raw materials in percentage by weight:
[0039] PBAT 75%, PPCP 20%, compatibilizer (p-phenylenediamine) 5%, granulation by twin-screw extrusion, granulation temperature: 140-160℃, the prepared mixed granules are blown by a film blowing machine, the blowing temperature: 160-175℃, to form a fully biodegradable mulch film product 1 with a thickness of 10 microns. The actual picture of the product 1 is as follows Figure 2 shown.
[0040] The infrared spectra of the raw materials PPCP, PBAT and product 1 in this example are as follows Figure 3-Figure 5 As shown, from Figure 5 It can be seen that at 1100cm -1 The peak at 2950 cm is attributed to the CC bonds of the aromatic rings, most of which come from the aromatic esters in PBAT. -1 The peaks at 1720 cm-1 represent the symmetric and asymmetric stretching of CH. -1 The characteristic peak at can be attributed to the absorption of all C=O groups of the ester bond, including all aliphatic esters and aromatic esters of PBAT and PPC. Figure 3 ) and PBAT( Figure 4 ) Compared with the addition of p-phenylenediamine to PBAT and PPCP, the FTIR spectrum of the product PBAT / PPCP / p-phenylenediamine 5% ground film is at 1517cm-1 The absorption peak at 3372 cm -1 The characteristic peak at can be attributed to the absorption of the CN group of the amide bond, which indicates that PBAT and PPCP react with p-phenylenediamine and form new amide bonds in the mulch film.
[0041] The melting curves of the raw materials PPCP, PBAT and product 1 in this example are as follows Figure 6 The crystallization curve is shown in Figure 7 As shown. Figure 6 and Figure 7 It can be seen that the addition of p-phenylenediamine increases the crystallization temperature of PBAT / PPCP by 50.05°C. This may be because p-phenylenediamine acts as a heterogeneous nucleation site in PBAT, reducing the nucleation free energy barrier and improving the crystallization ability. Blends with higher crystallization temperatures can be cooled and formed at higher temperatures, accelerating the solidification process of melt extrusion. It was found that the addition of p-phenylenediamine increased the melting temperature of PBAT / PPC-P by 4.2°C, indicating that p-phenylenediamine will hinder the molecular chain movement of PBAT and improve thermal stability.
[0042] Example 2
[0043] A PBAT / PPCP polymer film comprises the following raw materials in percentage by weight:
[0044] PBAT 70%, PPCP 20%, black masterbatch 5%, compatibilizer (p-phenylenediamine) 5%, granulation by twin-screw extrusion, granulation temperature: 140-160℃, the prepared mixed granules are blown by a film blowing machine, the blowing temperature is: 160-175℃, to form a fully biodegradable mulch film product 2 with a thickness of 10 microns.
[0045] Example 3
[0046] A PBAT / PPCP polymer film comprises the following raw materials in percentage by weight:
[0047] PBAT 67%, PPCP 30%, compatibilizer (p-phenylenediamine) 3%, granulated by twin-screw extrusion, granulation temperature: 130-150°C, the prepared mixed granules are blown by a film blowing machine, the blowing temperature is: 155-160°C, to form a fully biodegradable mulch film product 3 with a thickness of 10 microns.
[0048] Example 4
[0049] A PBAT / PPCP polymer film comprises the following raw materials in percentage by weight:
[0050] PBAT 62%, PPCP 30%, black masterbatch 5%, compatibilizer (p-phenylenediamine) 3%, granulation by twin-screw extrusion, granulation temperature: 130-150℃, the prepared mixed granules are blown by a film blowing machine, the blowing temperature is: 155-160℃, to form a fully biodegradable mulch film product 4 with a thickness of 10 microns.
[0051] Example 5
[0052] A PBAT / PPCP polymer film comprises the following raw materials in percentage by weight:
[0053] PBAT 74%, PPCP 25%, compatibilizer (p-phenylenediamine) 1%, granulation by twin-screw extrusion, granulation temperature: 125-145°C, the prepared mixed granules are blown by a film blowing machine, the blowing temperature is: 150-160°C, to form a fully biodegradable mulch film product 5 with a thickness of 10 microns.
[0054] Example 6
[0055] A PBAT / PPCP polymer film comprises the following raw materials in percentage by weight:
[0056] PBAT 69%, PPCP 25%, black masterbatch 5%, compatibilizer (p-phenylenediamine) 1%, granulated by twin-screw extrusion, granulation temperature: 125-145℃, the prepared mixed granules are blown by a film blowing machine, the blowing temperature is: 150-160℃, to form a fully biodegradable mulch film product 6 with a thickness of 10 microns.
[0057] Experimental example
[0058] 1. The performance of the fully biodegradable mulch film products prepared in Examples 1-6 was compared with that of the comparative film. The results are shown in Table 1.
[0059] The comparison film is made of pure PBAT as raw material through twin-screw extrusion granulation, the granulation temperature is 125-145°C, and the prepared mixed granules are blown by a film blowing machine, the blowing temperature is 150-160°C, to form a pure PBAT comparison film with a thickness of 12 microns.
[0060] The experimental standards and processes referenced by each experimental project are as follows:
[0061] 1. Mechanical properties (tensile, right-angle tear): According to the requirements of GB / T1040.1-2018 and QB / T1130-1991, a universal tensile testing machine was used to test the longitudinal tensile properties and longitudinal right-angle tear properties of the samples. In the tensile performance test experiment, the ground film was cut into long strips of 10mm wide and 130mm long, the clamp distance was set to 100mm, and the test speed was set to 200mm / min. In the right-angle tear performance test experiment, the ground film was cut into samples that met the standard requirements using a mold, the clamp distance was set to 100m, and the test speed was set to 200mm / min. Each sample was repeated 5 times, and the final result was taken as the average value.
[0062] 2. Water vapor transmission rate: According to GBT1037-1988, use a water vapor transmission rate tester to test the water vapor transmission rate of the sample. Use a sampler to cut the ground film into a circular sample with an area of 33.2c. Put the sample and an appropriate amount of ultrapure water into the sample rack and place it in the sample chamber of the water vapor transmission rate tester. Set the output air pressure of the system to 4MPa-5Pa, and the pressure of the automatic dry filter to 0.3MPa-0.35MPa. The test temperature and relative humidity are set to 38C and 90% respectively. Set 2 repetitions for each sample.
[0063] 3. Aging test: The ground film was aged according to the requirements of ASTM G155-2013. This experiment was carried out in a xenon lamp aging test chamber. The aging cycle was exposed to a 0.51w / (m2nm) xenon lamp UV light source for 100 hours, and the wavelength was set to 340nm. The distilled water spray program was used for 18min every 120min, and the cycle was repeated in sequence. After 100h aging treatment, the tensile properties and right-angle tear properties of the samples were tested.
[0064] 4. The functional period specifically refers to the time from when the mulch film is laid in the field to when the mulch film begins to initially degrade, that is, the period when the mulch film fully functions.
[0065] 5. The functional period of biodegradable mulch corresponds to the growth and development period of the crop. In the early stage of crop growth and development, the mulch's ability to increase temperature and retain moisture can promote crop development. Therefore, the longer the functional period of the mulch, the longer the growth promotion time for crops, and the more effective the growth and development of crops. The crop yield is specifically spring corn. This shows that the product has excellent water vapor barrier properties and mechanical properties, which can extend the functional period of the mulch, maintain sufficient water and heat conditions for a long time in the early stage of crop growth and development, and promote biological development. Crops have sufficient growth and development conditions in the early stage of development, and accumulate more nutrients. When mature, the yield is significantly increased compared to the comparison film with a shorter functional period.
[0066] Table 1
[0067]
[0068] It can be seen from Table 1 that compared with the mulch film prepared from a single raw material PBAT material, the products 1-5 prepared in the examples of the present application have more excellent performance in terms of tensile strength, water vapor permeability, right-angle tearing, etc. After being actually applied in the fields, they can function for a longer time and promote the increase in the yield of agricultural products.
[0069] 2. Explore the impact of compatibilizers on the products of this application.
[0070] In this experimental example, epoxy polymer compatibilizer SAG-008 is used as a comparative compatibilizer, and other raw materials, proportions and process steps are the same as in Example 1. The results show that both compatibilizers can react with PPCP and PBAT, but compared with the reaction time of the comparative compatibilizer (30 min), the reaction speed of the p-phenylenediamine compatibilizer (reaction time is 10 min) is faster, which can shorten the reaction time, and p-phenylenediamine reacts with PBAT to form an amide bond, and the structure is more stable. Therefore, p-phenylenediamine is more suitable as a compatibilizer for PBAT and PPC in this application.
[0071] In addition, the present application also uses other amine compatibilizers (such as ethylenediamine, etc.) for control experiments. The compatibilization effect is not as good as that of p-phenylenediamine. The reason is that p-phenylenediamine has a special symmetrical structure and is relatively active. At the same time, the benzene ring is affected by the amino group, which enhances the activity of hydrogen on the ortho-para position of the amino group on the benzene ring and is easily replaced. Therefore, the compatibilizer used for PBAT is easy to react with the ester group of PBAT to form an amide bond, thereby enhancing the compatibility of the PBAT resin.
[0072] In summary, a PBAT / PPC polymer film and a preparation method thereof and an application in the field of biodegradable mulch films according to an embodiment of the present application have the following advantages: based on the characteristics that both PBAT and PPCP, two degradable polyester materials, contain ester groups, the present application introduces p-phenylenediamine as a compatibilizer, and realizes segment embedding between PBAT and PPCP through amine ester exchange reaction (amine ester exchange reaction occurs in ester compounds and can exchange hydroxyl groups therein, wherein the hydroxyl groups of the ester reactants are replaced by the amino groups of the amine reactants to form compounds having amide bonds), thereby improving the compatibility between the two, and finally forming a stable new polymer that retains the advantages of both. After the new polymer is prepared into a degradable mulch film, it has comprehensive improvements in terms of blow molding, mechanical properties, water vapor barrier properties and functional period compared to the original single material.
[0073] The embodiments described above are part of the embodiments of the present application, rather than all of the embodiments. The detailed description of the embodiments of the present application is not intended to limit the scope of the present application for protection, but merely represents the selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work belong to the scope of protection of the present application.
Claims
1. A PBAT / PPCP polymer film, characterized in that: The PBAT / PPCP polymer film comprises the following raw materials in weight percentage: 65-75% of PBAT, 20-30% of PPCP and 1-5% of a compatibilizer; the compatibilizer is p-phenylenediamine.
2. A PBAT / PPCP polymer film according to claim 1, characterized in that: The raw materials of the PBAT / PPCP polymer film also include 1-5% masterbatch.
3. A method for preparing a PBAT / PPCP polymer film according to claim 1 or 2, characterized in that: The following steps are involved: S1, weighing each raw material, placing the raw material in a twin-screw extruder for granulation, and obtaining mixed granules; S2. Blowing the mixed particles through a film blowing machine to obtain a polymer film.
4. The method for preparing a PBAT / PPCP polymer film according to claim 3, characterized in that: The granulation temperature in the step S1 is 125-160°C.
5. The method for preparing a PBAT / PPCP polymer film according to claim 3, characterized in that: The temperature of the blow molding in the step S1 is 150-175°C.
6. The method for preparing a PBAT / PPCP polymer film according to claim 3, characterized in that: The thickness of the polymer film is 8-15 μm.
7. Use of the PBAT / PPCP polymer film as claimed in claim 1 or 2 in the field of biodegradable mulch films.
Citation Information
Cited By
Compatibilizer for blending PPCP / PBAT and preparation method of blend
CN120518826A
Controllable biodegradable high-strength polylactic acid composite mulching film and preparation method thereof
CN121671133A
Controllable biodegradable high-strength polylactic acid composite mulching film and preparation method thereof
CN121671133B