Sulfur-coated high-conductivity nanocomposite material, preparation method and aluminum ion battery

By adding sulfur atoms into high-conductivity nanocomposites and performing acid treatment and sulfur coating, the problem of low capacity of aluminum-ion batteries is solved, the capacity and cycle stability of the battery are improved, and the use of high-conductivity nanocomposites in aluminum-ion batteries is solved. Effective applications in batteries.

CN117239074BActive Publication Date: 2024-10-29CHINA ENERGY HYDROGEN STORAGE (BEIJING) ENERGY ENG RES INST CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311133000.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-04
Publication Date
2024-10-29
Estimated Expiration
2043-09-04

AI Technical Summary

Technical Problem

The energy storage capacity and potential of existing aluminum-ion batteries need to be improved. The lack of active intercalation sites in high-conductivity nanocomposites limits their application in aluminum batteries, resulting in a reduction in the capacity of aluminum-ion batteries.

Method used

By adding sulfur atoms into high-conductivity nanocomposites to increase their defects and active sites, and through acid treatment and sulfur coating technology, sulfur-coated high-conductivity nanocomposites are prepared to increase their electronic conductivity, thereby improving aluminum The capacity of an ion battery.

Benefits of technology

It effectively improves the capacity and cycle stability of aluminum-ion batteries, enhances ion conductivity, improves aluminum storage performance, and has a simple preparation process and has good application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117239074B_ABST
    Figure CN117239074B_ABST
Patent Text Reader

Abstract

The present invention relates to a sulfur-coated high-conductivity nano-composite material, a preparation method and an aluminum ion battery, and belongs to the technical field of aluminum ion batteries. The composite material is formed by sulfur coating the outer surface of a high-conductivity nano-material, and also includes the situation that sulfur enters the structure of the high-conductivity nano-material. In the composite material, the sulfur content is 0.2% to 3% of the atomic percentage of the high-conductivity nano-material. In the preparation method, the high-conductivity nano-material is first treated with acid; then, according to the performance characteristics of thiourea and sulfur powder, sulfur is coated on the high-conductivity nano-material by soaking first and then calcining or directly calcining to prepare the composite material. The present invention increases the defects and active sites of the high-conductivity nano-composite material by adding sulfur atoms to the high-conductivity nano-composite material, and further enhances the electronic conductivity, so that the aluminum storage performance of the high-conductivity nano-composite material is improved, thereby increasing the capacity of the aluminum ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a sulfur-coated high-conductivity nanocomposite material, a preparation method and an aluminum ion battery, and belongs to the technical field of aluminum ion batteries. Background Art

[0002] In recent years, as large-scale energy storage devices have gradually become a research hotspot in the field of electrochemistry, rechargeable aluminum-ion batteries (AIBs) are considered to be the most promising alternative to the currently mature lithium-ion batteries due to their large storage capacity, cost-effectiveness, safety, and environmental friendliness. -3 The volumetric capacity of lithium-ion batteries is 4 times that of lithium-ion batteries. However, due to the inherent gap between theoretical experiments and commercial applications, the energy storage capacity, battery potential and energy density need to be greatly improved.

[0003] High-conductivity nanocomposite materials are nanomaterials with high conductivity, such as carbon nanotube paper and carbon nanotube film. As low-cost commercial materials, they have high conductivity and mechanical strength and are widely used in new energy related industries. However, due to the lack of active intercalation sites, their aluminum storage performance is limited, resulting in a decrease in the capacity of aluminum ion batteries, which makes their application in aluminum batteries very limited.

[0004] Chinese patent ZL 201811019127.2 discloses the use of sulfur-doped carbon materials to improve the electrochemical performance of sodium-ion batteries. However, as trivalent ion batteries, aluminum-ion batteries have a charging and discharging mode that is quite different from that of sodium-ion batteries, and it is impossible to determine the gain effect of sulfur in aluminum-ion batteries. Summary of the invention

[0005] In view of this, in order to solve the problem of poor capacity performance of existing aluminum ion batteries, the purpose of the present invention is to provide a sulfur-coated high-conductivity nano-composite material, a preparation method and an aluminum ion battery; by adding sulfur atoms to the high-conductivity nano-composite material to increase the defects and active sites of the high-conductivity nano-composite material, and further enhance the electronic conductivity, the aluminum storage performance of the high-conductivity nano-composite material is improved, thereby improving the capacity of the aluminum ion battery.

[0006] To achieve the purpose of the present invention, the following technical solutions are provided.

[0007] A sulfur-coated high-conductivity nano-composite material, wherein the composite material is formed by sulfur coating the outer surface of a high-conductivity nano-material, and further includes the situation where sulfur enters the structure of the high-conductivity nano-material.

[0008] In the composite material, the content of sulfur is 0.2% to 3% of the atomic percentage of the high-conductivity nanomaterial.

[0009] The high-conductivity nanomaterial is a nanocarbon material with high conductivity, and the conductivity is 2×10 3 S / m~2×10 5 S / m.

[0010] Preferably, the highly conductive nanomaterial is a carbon nanotube (CNT) having a thickness of 10 μm to 90 μm.

[0011] A method for preparing the sulfur-coated high-conductivity nanocomposite material of the present invention comprises the following steps:

[0012] (1) The high-conductivity nanomaterial is completely immersed in an acid solution and allowed to stand for acid treatment. After the treatment is completed, the acid solution is removed by washing and the material is dried to obtain the high-conductivity nanomaterial after the acid treatment.

[0013] Preferably, the acid solution is a nitric acid solution, a hydrochloric acid solution or a sulfuric acid solution; more preferably, the acid solution is a 68% by mass concentrated nitric acid solution, a 36% to 38% by mass concentrated hydrochloric acid solution or a 70% by mass concentrated sulfuric acid solution.

[0014] Furthermore, the preferred acid solution is a concentrated nitric acid solution with a mass fraction of 68%.

[0015] The acid treatment is preferably carried out in a closed container to avoid volatilization of the acid solution.

[0016] Preferably, when the acid solution is a concentrated nitric acid solution with a mass fraction of 68%, it is allowed to stand for more than 12 hours.

[0017] The acid can be removed by cleaning with water and ethanol respectively.

[0018] The preferred drying temperature is 75°C to 85°C, and the drying can be carried out in an oven.

[0019] (2) treating the acid-treated high-conductivity nanomaterial obtained in step (1) with a sulfur source to obtain a sulfur-coated high-conductivity nanocomposite material according to the present invention.

[0020] The sulfur source is thiourea or sulfur powder.

[0021] ① When the sulfur source is thiourea, the treatment method is:

[0022] Fully dissolving thiourea with a solvent to prepare a thiourea solution, completely immersing the acid-treated high-conductivity nanomaterial in the thiourea solution, allowing it to stand, then taking it out and drying it to obtain the immersed material;

[0023] The soaked material is calcined under the protection of an inert gas or sulfur atmosphere, the temperature is raised to 600°C to 800°C and calcined at a constant temperature for 2h to 5h, and the heating rate is less than or equal to 2.5°C / min.

[0024] The mass ratio of the high-conductivity nanomaterial to thiourea is 1:(0.5-3).

[0025] The preferred mass ratio of high-conductivity nanomaterials to thiourea is 1:1.5

[0026] The solvent of the thiourea solution is water, ethanol, ether or acetone, etc., which can dissolve thiourea. The less the amount of solvent used, the better if thiourea can be dissolved. The preferred solvent of the thiourea solution is acetone, which can better soak the highly conductive nanomaterial.

[0027] Preferably, the thiourea is fully dissolved in the solvent by stirring to form a thiourea solution, the stirring speed is 350 r / min to 650 r / min, and the stirring time is 8 min to 15 min.

[0028] Furthermore, it is preferred to use ultrasound for dispersion to fully dissolve the thiourea in the solvent to form a thiourea solution, the power of the ultrasound is 600 mph, and the time is not less than 5 minutes.

[0029] It is preferred to seal the opening of the soaking container with a plastic wrap with holes when leaving it at rest, which can prevent the solution from evaporating and draining water.

[0030] The calcination can be carried out in a tubular furnace.

[0031] ② When the sulfur source is sulfur powder, the treatment method is:

[0032] The acid-treated high-conductivity nanomaterial and sulfur powder are calcined under the protection of an inert gas or sulfur atmosphere, and the temperature is raised to 110° C. to 140° C. for constant calcination for 2 h to 5 h, with a heating rate of less than or equal to 2.5° C. / min.

[0033] The mass ratio of the high-conductivity nanomaterial to the sulfur powder is 1:(1-3).

[0034] The calcination can be carried out in a tubular furnace.

[0035] An aluminum ion battery, wherein the positive electrode material of the battery is the sulfur-coated high-conductivity nanocomposite material of the present invention.

[0036] Preferably, the negative electrode of the aluminum ion battery is an aluminum foil with a thickness of 30 μm to 100 μm.

[0037] Preferably, the separator of the aluminum ion battery is at least one of a glass fiber membrane, a polypropylene (PP) membrane and a polyethylene (PE) membrane.

[0038] Beneficial Effects

[0039] (1) The present invention provides a sulfur-coated high-conductivity nanocomposite material. The composite positive electrode material increases the defects and active sites of the high-conductivity nanocomposite material by adding sulfur atoms, while further enhancing the ionic conductivity, thereby effectively improving the aluminum storage performance and the capacity of the aluminum ion battery.

[0040] (2) The present invention provides a sulfur-coated high-conductivity nano-composite material. The sulfur content in the composite positive electrode material has a very important influence on its performance. Therefore, the range of sulfur doping is limited. If the amount of sulfur added is too little, the sulfur atoms are coated too little and unevenly, which will reduce the number of active sites and reduce the capacity; if the amount added is too much, the structure of the high-conductivity nano-material will be destroyed and the impedance will increase.

[0041] (3) The present invention provides a sulfur-coated high-conductivity nanocomposite material, wherein the three-dimensional structure of the high-conductivity nanomaterial can accelerate the speed of ion transmission during long cycles of the composite positive electrode material.

[0042] (4) The present invention provides a method for sulfur-coated high-conductivity nanocomposite materials, wherein the high-conductivity nanomaterial is first treated with acid in order to better coat the sulfur and remove the influence of moisture and other impurities; then, sulfur is coated on the high-conductivity nanomaterial by different methods according to the performance characteristics of different sulfur sources, thereby preparing the sulfur-coated high-conductivity nanocomposite material described in the present invention.

[0043] (5) The present invention provides a method for preparing a sulfur-coated high-conductivity nanocomposite material. The method has a simple preparation process and is suitable for promotion and has good application prospects.

[0044] (6) The present invention provides an aluminum ion battery, wherein the positive electrode material of the battery is the sulfur-coated high-conductivity nanocomposite material of the present invention, which has a high initial specific capacity and a low capacity decay rate, and has good cycle stability, rate performance and coulombic efficiency. This is because the addition of sulfur atoms increases the defects and active sites of the high-conductivity nanomaterial, while further enhancing the ionic conductivity, effectively improving the problem of low capacity of the aluminum ion battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 This is a scanning electron microscope (SEM) image of the final product prepared in Example 1.

[0046] Figure 2 The X-ray photoelectron spectroscopy (XPS) diagram of the final product prepared in Example 1.

[0047] Figure 3 This is the near infrared test image of the final product prepared in Example 1.

[0048] Figure 4This is a test diagram of the cycling performance of an aluminum ion battery using the final product prepared in Example 1 as the positive electrode. DETAILED DESCRIPTION

[0049] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments and drawings.

[0050] In the following embodiments, the following detection is involved:

[0051] (1) Scanning electron microscopy (SEM)

[0052] The microstructure of the final product was observed using a field emission scanning electron microscope (FEIQuanta 600) with an accelerating voltage of 25 kV.

[0053] (2) X-ray photoelectron spectroscopy (XPS)

[0054] A non-destructive measurement technology that detects material surface information by incident on the surface of the final product with a photon beam at a depth of 3nm to 10nm. It can be used to qualitatively and quantitatively analyze the elemental composition and content of the material surface, as well as analyze the chemical valence, chemical bonds and other information of the elements.

[0055] (3) Fourier transform infrared spectroscopy (FTIR)

[0056] The surface of the final product is detected using the principle of infrared radiation.

[0057] (4) Aluminum ion battery performance testing

[0058] Aluminum ion batteries are assembled as follows:

[0059] Aluminum ion batteries were assembled in a glove box with an argon atmosphere and water and oxygen concentrations less than 0.1 ppm. The positive electrode, glass fiber separator, and negative electrode were placed in a Swagelok battery mold in order for lamination, and the electrolyte was dripped into the mold to fully wet the glass fiber separator, and then the mold was tightened; the electrolyte was an ionic liquid electrolyte 1-ethyl-3-methylimidazole chloride ([EMIm]Cl) mixed with anhydrous aluminum chloride (AlCl3) in a molar ratio of 1.3:1;

[0060] The final products prepared in the examples and comparative examples, namely sulfur-coated high-conductivity nanocomposites (CNT@S) and pure aluminum foil, were used as electrodes to assemble aluminum ion batteries. The electrochemical performance of the aluminum ion batteries was tested using the Land system, and the test data was recorded and analyzed using Origin.

[0061] Charge / discharge cycle performance test: It is one of the common methods for detecting the electrochemical performance of electrode materials. The charge / discharge cycle performance test of the following examples and comparative examples uses a CT2001A battery test system produced by Wuhan Blue Electric Electronics Co., Ltd., and the test voltage window range is 0.3V to 2.2V.

[0062] Example 1

[0063] (1) Slowly drop a 68% concentrated nitric acid solution into a glass petri dish containing a highly conductive nanomaterial until the carbon nanotubes are completely immersed in the nitric acid solution, wherein the highly conductive nanomaterial is a square carbon nanotube paper weighing 9.56 mg and having a thickness of 60 μm to 90 μm. Wrap the glass petri dish with a thin aluminum foil as a sealed container to prevent the nitric acid from volatilizing, and let it stand for 24 hours for acid treatment. After the treatment is completed, take out the acid-treated sample, wash it twice with deionized water, and then wash it once with ethanol to remove the acid solution, and then put it in an oven and dry it at 80°C for 12 hours to obtain the acid-treated highly conductive nanomaterial;

[0064] (2) 14.34 mg of thiourea and 8 ml of acetone were mixed and stirred and ultrasonically treated at a stirring speed of 650 r / min, a stirring time of 10 min, an ultrasonic power of 600 mph, and an ultrasonic time of 8 min to fully dissolve the thiourea in acetone to form a thiourea solution; the mass ratio of the high-conductivity nanomaterial to thiourea was 1:1.5;

[0065] The acid-treated high-conductivity nanomaterial is placed in a glass culture dish, and the thiourea solution is slowly added dropwise into the glass culture dish until the acid-treated high-conductivity nanomaterial is completely immersed in the thiourea solution. The glass culture dish is sealed with a plastic wrap with holes, and the glass culture dish is left to stand for 12 hours, and then taken out and dried to obtain the immersed material;

[0066] (3) The soaked material was placed in a tubular furnace, and under the protection of an argon atmosphere, the temperature was increased to 700° C. at a heating rate of 2.5° C. / min, and constant temperature calcined for 3 h to prepare the final product.

[0067] The final product prepared in this example was tested as follows:

[0068] (1) Scanning electron microscopy (SEM)

[0069] Figure 1 This is the SEM image of the final product, which shows that in the final product after the carbon nanotubes are calcined, the diameter of each carbon nanotube is 0.1μm~0.2μm, and the surface morphology of the final product still maintains the original structure of the carbon nanotubes, and sulfur is evenly coated on its network, without obvious large clusters of sulfur deposition morphology.

[0070] (2) X-ray photoelectron spectroscopy (XPS)

[0071] Figure 2 : is the XPS graph of the final product, which has an obvious S2p ​​characteristic peak, indicating that sulfur is successfully coated on the high-conductivity nanomaterial in this embodiment; the XPS result shows that the doping amount of sulfur is 0.59% of the atomic percentage of the high-conductivity nanomaterial.

[0072] (3) Fourier transform infrared spectroscopy (FTIR)

[0073] Figure 3 The FTIR spectrum of the final product shows that -1 and 1090cm -1 The stretching vibrations of the CS and SO bonds can be observed, further indicating that sulfur has entered the structure of the highly conductive nanomaterial.

[0074] From the above test results, it can be seen that the final product of this embodiment is a sulfur-coated high-conductivity nanocomposite material (CNT@S), which is formed by sulfur coating the outer surface of the high-conductivity nanomaterial, and further includes the situation where sulfur enters the structure of the high-conductivity nanomaterial.

[0075] (4) Aluminum ion battery performance testing

[0076] The final product prepared in this example was used as the positive electrode to assemble an aluminum ion battery, and the battery cycle performance test was performed as follows:

[0077] The constant current charge and discharge test of the battery was carried out at room temperature using a BluePower CT2001A multi-channel battery test system within a fixed voltage range of 0.3V to 2.2V. Figure 4 This is the aluminum ion battery cycle performance test diagram. It can be seen from the figure that at 500mA g -1 At the current density of , the first cycle charge and discharge capacities are 340 mAh g -1 and 76mAh g -1 ; At the same time, the stability is good, gradually stabilized after 100 cycles, and maintained at 70mA g -1 .

[0078] Example 2

[0079] The concentrated nitric acid solution in step (1) of Example 1 was replaced with a concentrated hydrochloric acid solution with a mass fraction of 37%, and the other steps and conditions remained unchanged.

[0080] The final product prepared in this example was tested as follows:

[0081] (1) Scanning electron microscopy (SEM)

[0082] SEM results show that in the final product, the diameter of each carbon nanotube is 0.1μm~0.2μm, and the surface morphology of the final product still maintains the original structure of the carbon nanotubes, and sulfur is evenly coated on its network, without obvious large clusters of sulfur deposition morphology.

[0083] (2) X-ray photoelectron spectroscopy (XPS)

[0084] The XPS result shows an obvious S2p ​​characteristic peak, indicating that sulfur is successfully coated on the high-conductivity nanomaterial in this embodiment; the doping amount of sulfur is 0.4% of the atomic percentage of the high-conductivity nanomaterial.

[0085] (3) Fourier transform infrared spectroscopy (FTIR)

[0086] FTIR results showed that the -1 and 1090cm -1 The stretching vibrations of the CS and SO bonds can be observed, further indicating that sulfur has entered the structure of the highly conductive nanomaterial.

[0087] From the above test results, it can be seen that the final product of this embodiment is a sulfur-coated high-conductivity nanocomposite material (CNT@S), which is formed by sulfur coating the outer surface of the high-conductivity nanomaterial, and further includes the situation where sulfur is coated into the structure of the high-conductivity nanomaterial.

[0088] (4) Aluminum ion battery performance testing

[0089] The final product prepared in this example was used as the positive electrode to assemble an aluminum ion battery, and the battery cycle performance test was performed as follows:

[0090] The constant current charge and discharge test of the battery was carried out at room temperature using the Blue Power CT2001A multi-channel battery test system in a fixed voltage range of 0.3V to 2.2V. The cycle performance test results of the aluminum ion battery showed that at 500mA g -1 At the current density of , the first cycle charge and discharge capacities are 320mAh g -1 and 64mAh g -1 ; At the same time, the stability is good, gradually stabilized after 100 cycles, and maintained at 58mA g -1 ; Slightly inferior to the performance of the aluminum ion battery in Example 1.

[0091] Example 3

[0092] The mass ratio of the highly conductive nanomaterial to thiourea in step (2) of Example 1 was changed from 1:1.5 to 1:0.8, while other steps and conditions remained unchanged.

[0093] The final product prepared in this example was tested as follows:

[0094] (1) Scanning electron microscopy (SEM)

[0095] SEM results show that in the final product, the diameter of each carbon nanotube is 0.1μm~0.2μm, and the surface morphology of the final product still maintains the original structure of the carbon nanotubes, and most of its network is evenly coated with sulfur, without obvious large clusters of sulfur deposition morphology.

[0096] (2) X-ray photoelectron spectroscopy (XPS)

[0097] The XPS result shows an obvious S2p ​​characteristic peak, indicating that sulfur is successfully coated on the high-conductivity nanomaterial in this embodiment; the doping amount of sulfur is 0.28% of the atomic percentage of the high-conductivity nanomaterial.

[0098] (3) Fourier transform infrared spectroscopy (FTIR)

[0099] FTIR results showed that the -1 and 1090cm -1 The stretching vibrations of the CS and SO bonds can be observed, further indicating that sulfur has entered the structure of the highly conductive nanomaterial.

[0100] From the above test results, it can be seen that the final product of this embodiment is a sulfur-coated high-conductivity nanocomposite material (CNT@S), which is formed by sulfur coating the outer surface of the high-conductivity nanomaterial, and further includes the situation where sulfur enters the structure of the high-conductivity nanomaterial.

[0101] (4) Aluminum ion battery performance testing

[0102] The final product prepared in this example was used as the positive electrode to assemble an aluminum ion battery, and the battery cycle performance test was performed as follows:

[0103] The constant current charge and discharge test of the battery was carried out at room temperature, using the Blue Power CT2001A multi-channel battery test system, within a fixed voltage range of 0.3V to 2.2V. The cycle performance test results of the aluminum ion battery showed that at 500mA g -1 At a current density of 2.5, the first cycle charge and discharge capacities are 299 mAh g -1 and 66mAh g -1 ; At the same time, the stability is good, gradually stabilized after 130 cycles, and maintained at 54mA g -1 ; Slightly inferior to the cycle performance of the aluminum ion battery in Examples 1 and 2.

[0104] Example 4

[0105] (1) Same as step (1) of Example 1;

[0106] (2) 4.4 mg of sulfur powder was placed in a porcelain boat containing high-conductivity nanomaterials; the mass ratio of high-conductivity nanomaterials to sulfur powder was 1:1;

[0107] The high-conductivity nanomaterial and sulfur powder were placed in a tubular furnace, and under the protection of an argon atmosphere, the temperature was increased to 140°C at a heating rate of 2.5°C / min, and the mixture was calcined at a constant temperature for 3 hours to prepare the final product.

[0108] The final product prepared in this example was tested as follows:

[0109] (1) Scanning electron microscopy (SEM)

[0110] SEM results show that in the final product, the diameter of each carbon nanotube is 0.1μm~0.2μm, and the surface morphology of the final product still maintains the original structure of the carbon nanotubes, and sulfur is evenly coated on its network, without obvious large clusters of sulfur deposition morphology.

[0111] (2) X-ray photoelectron spectroscopy (XPS)

[0112] The XPS result shows an obvious S2p ​​characteristic peak, indicating that sulfur is successfully coated on the high-conductivity nanomaterial in this embodiment; the doping amount of sulfur is 0.5% of the atomic percentage of the high-conductivity nanomaterial.

[0113] (3) Fourier transform infrared spectroscopy (FTIR)

[0114] FTIR results showed that the -1 and 1090cm -1 The stretching vibrations of the CS and SO bonds can be observed, further indicating that sulfur has entered the structure of the highly conductive nanomaterial.

[0115] From the above test results, it can be seen that the final product of this embodiment is a sulfur-coated high-conductivity nanocomposite material (CNT@S), which is formed by sulfur coating the outer surface of the high-conductivity nanomaterial, and further includes the situation where sulfur enters the structure of the high-conductivity nanomaterial.

[0116] (4) Aluminum ion battery performance testing

[0117] The final product prepared in this example was used as the positive electrode to assemble an aluminum ion battery, and the battery cycle performance test was performed as follows:

[0118] The constant current charge and discharge test of the battery was carried out at room temperature, using the Blue Power CT2001A multi-channel battery test system, within a fixed voltage range of 0.3V to 2.2V. The cycle performance test results of the aluminum ion battery showed that at 500mA g -1 At a current density of , the first cycle charge and discharge capacities are 328 mAh g -1and 69mAh g -1 ; At the same time, the stability is good, gradually stabilized after 100 cycles, and maintained at 57mAg -1 ; Slightly inferior to the cycle performance of the aluminum ion battery in Example 1.

[0119] Example 5

[0120] The calcination temperature in step (2) of Example 4 was changed from 140° C. to 110° C., while other steps and conditions remained unchanged.

[0121] The final product prepared in this example was tested as follows:

[0122] (1) Scanning electron microscopy (SEM)

[0123] SEM results show that in the final product, the diameter of each carbon nanotube is 0.1μm~0.2μm, and the surface morphology of the final product still maintains the original structure of the carbon nanotubes, and sulfur is evenly coated on its network. There is no obvious large-scale clustered sulfur deposition morphology. A small amount of clustered S appears, which may be due to the low temperature, resulting in the incomplete gasification of S.

[0124] (2) X-ray photoelectron spectroscopy (XPS)

[0125] The XPS result shows an obvious S2p ​​characteristic peak, indicating that sulfur is successfully coated on the high-conductivity nanomaterial in this embodiment; the doping amount of sulfur is 0.44% by atomic percentage of the high-conductivity nanomaterial.

[0126] (3) Fourier transform infrared spectroscopy (FTIR)

[0127] FTIR results showed that the -1 and 1090cm -1 The stretching vibrations of the CS and SO bonds can be observed, further indicating that sulfur has entered the structure of the highly conductive nanomaterial.

[0128] From the above test results, it can be seen that the final product of this embodiment is a sulfur-coated high-conductivity nanocomposite material (CNT@S), which is formed by sulfur coating the outer surface of the high-conductivity nanomaterial, and further includes the situation where sulfur enters the structure of the high-conductivity nanomaterial.

[0129] (4) Aluminum ion battery performance testing

[0130] The final product prepared in this example was used as the positive electrode to assemble an aluminum ion battery, and the battery cycle performance test was performed as follows:

[0131] The constant current charge and discharge test of the battery was carried out at room temperature, using the Blue Power CT2001A multi-channel battery test system, within a fixed voltage range of 0.3V to 2.2V. The cycle performance test results of the aluminum ion battery showed that at 500mAg -1 At a current density of 2.5 mAh g, the first cycle charge and discharge capacities are 285 mAh g -1 and 57mAh g -1 ; At the same time, the stability is good, gradually stabilized after 140 cycles, and maintained at 44mAg -1 ; Slightly inferior to the cycle performance of the aluminum ion battery in Example 4.

[0132] Comparative Example 1

[0133] (1) Same as step (1) of Example 1;

[0134] (2) The acid-treated high-conductivity nanomaterial is placed in a tubular furnace, and under the protection of an argon atmosphere, the temperature is increased to 700° C. at a heating rate of 2.5° C. / min, and the material is calcined at a constant temperature for 3 h to obtain the final product.

[0135] The final product prepared in this comparative example was tested as follows:

[0136] (1) Scanning electron microscopy (SEM)

[0137] SEM results show that in the final product, the diameter of each carbon nanotube is about 0.1μm to 0.2μm, and the surface morphology of the final product still maintains the original structure of the carbon nanotube.

[0138] (2) X-ray photoelectron spectroscopy (XPS)

[0139] XPS results show that there is an O1s characteristic peak but no S2p characteristic peak, which indicates that the highly conductive nanomaterial was successfully oxidized in this embodiment.

[0140] It can be seen from the above test results that the final product obtained in this comparative example is an oxidized material.

[0141] (3) Aluminum ion battery performance testing

[0142] The final product prepared in this comparative example was used as the positive electrode to assemble an aluminum ion battery, and the battery cycle performance test was performed as follows:

[0143] The constant current charge and discharge test of the battery was carried out at room temperature, using the Blue Power CT2001A multi-channel battery test system, within a fixed voltage range of 0.3V to 2.2V. The cycle performance test results of the aluminum ion battery showed that at 500mAg -1 At the current density of , the first cycle charge and discharge capacities are 184 mAh g -1 and 42mAh g -1; After 100 cycles, it gradually stabilized and remained at 37mA g -1 ; It is significantly lower than the cycle performance of the aluminum ion batteries in Examples 1 to 5.

[0144] Comparative Example 2

[0145] The mass ratio of the high-conductivity nanomaterial to thiourea in step (2) of Example 1 was changed from 1:1.5 to 1:15, while other steps and conditions remained unchanged.

[0146] The final product prepared in this comparative example was tested as follows:

[0147] (1) Scanning electron microscopy (SEM)

[0148] SEM results show that in the final product, the diameter of each carbon nanotube is about 0.1μm to 0.2μm, and the original structure of the carbon nanotubes on the surface of the final product is partially destroyed, with large clusters of sulfur deposits appearing.

[0149] (2) X-ray photoelectron spectroscopy (XPS)

[0150] XPS results show that there is an obvious S2p ​​characteristic peak, indicating that sulfur is successfully coated on the high-conductivity nanomaterial in this embodiment; the doping amount of sulfur is 3.3% of the atomic percentage of the high-conductivity nanomaterial.

[0151] (3) Fourier transform infrared spectroscopy (FTIR)

[0152] FTIR results show: at 528cm -1 and 1090cm -1 The stretching vibrations of the CS and SO bonds can be observed, further indicating that sulfur is coated on the highly conductive nanomaterial structure.

[0153] (4) Aluminum ion battery performance testing

[0154] The final product prepared in this comparative example was used as the positive electrode to assemble an aluminum ion battery, and the battery cycle performance test was performed as follows:

[0155] The constant current charge and discharge test of the battery was carried out at room temperature, using the Blue Power CT2001A multi-channel battery test system, within a fixed voltage range of 0.3V to 2.2V. The cycle performance test results of the aluminum ion battery showed that at 500mAg -1 At the current density of , the first cycle charge and discharge capacities are 213 mAh g -1 and 45mAh g -1 ; After 300 cycles, it gradually stabilized and remained at 30mA g -1; It is significantly lower than the cycle performance of the aluminum ion battery in Examples 1 to 5; The proportion of sulfur in this comparative example is too high, which may destroy the original carbon structure of CNTs and deteriorate the cycle stability.

[0156] Comparative Example 3

[0157] The calcination temperature in step (3) of Example 1 was changed from 700° C. to 500° C., while the other steps and conditions remained unchanged.

[0158] The final product prepared in this comparative example was tested as follows:

[0159] (1) Scanning electron microscopy (SEM)

[0160] SEM results show that in the final product, the diameter of each carbon nanotube is 0.1μm to 0.2μm, and the surface morphology of the final product still maintains the original structure of the carbon nanotube, with a small amount of sulfur coated on its network.

[0161] (2) X-ray photoelectron spectroscopy (XPS)

[0162] XPS results show that there is no obvious S2p ​​characteristic peak.

[0163] (3) Fourier transform infrared spectroscopy (FTIR)

[0164] FTIR results show: at 528cm -1 and 1090cm -1 The stretching vibrations of CS and SO bonds can be observed, indicating that sulfur has entered the structure of the highly conductive nanomaterial.

[0165] (4) Aluminum ion battery performance testing

[0166] The final product prepared in this comparative example was used as the positive electrode to assemble an aluminum ion battery, and the battery cycle performance test was performed as follows:

[0167] The constant current charge and discharge test of the battery was carried out at room temperature, using the Blue Power CT2001A multi-channel battery test system, within a fixed voltage range of 0.3V to 2.2V. The cycle performance test results of the aluminum ion battery showed that at 500mAg -1 At the current density of , the first cycle charge and discharge capacities are 98 mAh g -1 and 32mAh g -1 ; After 100 cycles, it gradually stabilized and remained at 25mA g -1 ; The cycle performance of the aluminum ion battery in Examples 1 to 5 is significantly lower than that in Examples 1 to 5; the calcination temperature in this comparative example is too low, which may result in S not being completely coated or entering the high-conductivity nanomaterial, and the structure of CNTs being destroyed, resulting in a lower charge and discharge capacity.

[0168] Comparative Example 4

[0169] The calcination temperature in step (2) of Example 4 was changed from 140° C. to 300° C., while the other steps and conditions remained unchanged.

[0170] The final product prepared in this comparative example was tested as follows:

[0171] (1) Scanning electron microscopy (SEM)

[0172] SEM results show that in the final product, the diameter of each carbon nanotube is about 0.1μm to 0.2μm, and the surface morphology of the final product still maintains the original structure of the carbon nanotube, but no obvious coating is seen.

[0173] (2) X-ray photoelectron spectroscopy (XPS)

[0174] XPS results show that there is no obvious S2p ​​characteristic peak.

[0175] (3) Aluminum ion battery performance testing

[0176] The final product prepared in this comparative example was used as the positive electrode to assemble an aluminum ion battery, and the battery cycle performance test was performed as follows:

[0177] The constant current charge and discharge test of the battery was carried out at room temperature using the Blue Power CT2001A multi-channel battery test system in a fixed voltage range of 0.3V to 2.2V. The cycle performance test results of the aluminum ion battery showed that at 500mA g -1 At the current density of , the first cycle charge and discharge capacities are 178 mAh g -1 and 39mAh g -1 ; After 100 cycles, it gradually stabilized and remained at 33mAg -1 ; The calcination temperature in this comparative example is slightly higher, and the performance is significantly lower than the cycle performance of the aluminum ion battery in Examples 1 to 5.

[0178] The above embodiments are only preferred embodiments of the present invention and do not limit the present invention in any form. Any simple modifications, equivalent changes and modifications made to the above implementation methods within the technical essence of the present invention are within the protection scope of the technical solution of the present invention.

Claims

1. A sulfur-coated high-conductivity nanocomposite material, characterized in that: The composite material is formed by sulfur coating the outer surface of the high-conductivity nanomaterial, and also includes the case where sulfur enters the structure of the high-conductivity nanomaterial; The high-conductivity nanomaterial has an electrical conductivity of 2×10 3 S / m~2×10 5 S / m carbon nanotubes; In the composite material, the content of sulfur is 0.2% to 3% of the atomic percentage of the highly conductive nanomaterial; The composite material is prepared by the following method: (1) completely immersing the high-conductivity nanomaterial in an acid solution and allowing it to stand for acid treatment. After the treatment is completed, washing to remove the acid solution and drying to obtain the high-conductivity nanomaterial after acid treatment; (2) treating the acid-treated high-conductivity nanomaterial obtained in step (1) with a sulfur source to obtain a sulfur-coated high-conductivity nanocomposite material; Wherein, the sulfur source is thiourea or sulfur powder; ① When the sulfur source is thiourea, the treatment method is: Fully dissolving thiourea with a solvent to prepare a thiourea solution, completely immersing the acid-treated high-conductivity nanomaterial in the thiourea solution, allowing it to stand, then taking it out and drying it to obtain the immersed material; The soaked material is heated to 600℃~800℃ and calcined at a constant temperature for 2h~5h under the protection of an inert gas or sulfur atmosphere, with a heating rate of less than or equal to 2.5℃ / min; The mass ratio of the high-conductivity nanomaterial to thiourea is 1: (0.5~3); ② When the sulfur source is sulfur powder, the treatment method is: The acid-treated high-conductivity nanomaterial and sulfur powder are heated to 110° C. to 140° C. and calcined at a constant temperature for 2 h to 5 h under the protection of an inert gas or sulfur atmosphere, with a heating rate of less than or equal to 2.5° C. / min; The mass ratio of high-conductivity nanomaterials to sulfur powder is 1:(1~3).

2. The sulfur-coated high-conductivity nanocomposite material according to claim 1, characterized in that: The thickness of the carbon nanotubes is 10 μm to 90 μm.

3. The sulfur-coated high-conductivity nanocomposite material according to claim 1, characterized in that: In step (1), the acid solution is a nitric acid solution, a hydrochloric acid solution or a sulfuric acid solution.

4. The sulfur-coated high-conductivity nanocomposite material according to claim 1, characterized in that: In step (1), the acid treatment is carried out in a sealed container; in step (2), the opening of the container used for soaking is sealed with a plastic wrap with holes while standing.

5. The sulfur-coated high-conductivity nanocomposite material according to claim 1, characterized in that: In step (1), water and ethanol are used to clean and remove the acid solution respectively; the drying temperature is 75°C to 85°C; in step (2), the solvent of the thiourea solution is water, ethanol, ether or acetone; the thiourea is fully dissolved in the solvent by stirring to form a thiourea solution, the stirring speed is 350r / min to 650r / min, and the stirring time is 8min to 15min; or ultrasonic dispersion is used to fully dissolve the thiourea in the solvent to form a thiourea solution, the ultrasonic power is 600mph, and the time is not less than 5min.

6. A sulfur-coated high-conductivity nanocomposite material according to any one of claims 1 to 5, characterized in that: In step (1), the acid solution is a concentrated nitric acid solution with a mass fraction of 68%, a concentrated hydrochloric acid solution with a mass fraction of 36% to 38%, or a concentrated sulfuric acid solution with a mass fraction of 70%. When the acid solution is a concentrated nitric acid solution with a mass fraction of 68%, it is left to stand for more than 12 hours. In step (2), the mass ratio of the high-conductivity nanomaterial to thiourea is 1:1.5; and the solvent of the thiourea solution is acetone.

7. An aluminum ion battery, characterized in that: The positive electrode material of the battery is the sulfur-coated high-conductivity nanocomposite material as claimed in claim 1 or 2.

8. An aluminum ion battery according to claim 7, characterized in that: The negative electrode of the aluminum ion battery is an aluminum foil with a thickness of 30 μm to 100 μm; The separator of the aluminum ion battery is at least one of a glass fiber membrane, a polypropylene membrane and a polyethylene membrane.

Citation Information

Patent Citations

  • Preparation method of a sulfur-doped carbon micron tube, a sulfur-doped carbon micron tube and an application thereof

    CN109273272A

  • Porous carbon coated carbon-sulfur composite positive pole and aluminum secondary battery

    CN204156010U