A method for producing hydrogen by bipolar oxidation of furfural by acid-base asymmetric coupling
Through the bipolar hydrogen production method of furfural oxidation by acid-base asymmetric coupling, furfural oxidation reaction is used to replace the anode oxygen evolution reaction, reducing the energy consumption of electrolytic hydrogen production, and achieving the coordinated production of high-value-added chemicals, solving the existing solutions The high energy consumption and explosion risk of electrolyzed hydrogen production in the technology.
Patent Information
- Application Number
- CN202311189294.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-15
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-09-15
AI Technical Summary
In the existing electrolytic hydrogen production technology, the slow kinetic reaction of the anode oxygen evolution reaction leads to high energy consumption, and the power consumption of traditional alkaline and proton membrane electrolytic cells is greater than 4kWh when producing hydrogen, which poses a risk of explosion.
The hydrogen production method of furfural oxidation bipolar method is adopted by acid-base asymmetric coupling of furfural oxidation bipolar. By filling the anode reaction chamber with a mixed solution containing furfural and alkali, filling the cathode reaction chamber with an acid solution, and applying a voltage of 0.35 to 0.50V using a DC power supply, furfural chloride is used to apply a voltage of 0.35 to 0.50V. Dehydrogenation and furoic acid are generated by Tafel reaction to produce hydrogen, reducing the energy consumption of electrolytic hydrogen production.
It realizes the reduction of the energy consumption of electrolytic hydrogen production under the low voltage range, reduces the energy consumption of the anode, and reduces the production cost through the collaborative production of high-value-added chemicals, and improves Faraday efficiency and market application prospects.
Smart Images

Figure CN117248218B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to electrolytic hydrogen production and biomass conversion technology, and in particular to a method for producing hydrogen through bipolar oxidation of furfural by acid-base asymmetric coupling. Background Art
[0002] Hydrogen (H2) has the characteristics of high calorific value (143kJ / g) and zero carbon emission of combustion products, and is regarded as an ideal green and clean energy. Compared with the carbon emission problem in the process of hydrogen production by reforming fossil fuels, water electrolysis hydrogen production technology can achieve zero-emission hydrogen production. And green hydrogen produced by coupling with renewable energy can realize energy redistribution in time and space, and green hydrogen production has become an important global energy carrier.
[0003] The water electrolysis process includes two half reactions: the hydrogen evolution reaction (HER) at the cathode and the oxygen evolution reaction (OER) at the anode. Among them, the cathode HER is a relatively simple two-electron transfer process that can occur at a lower potential. However, the anode OER process requires a four-electron transfer process, and its kinetic reaction is slow, which greatly reduces the energy efficiency of hydrogen production. Traditional alkaline electrolyzers and proton membrane electrolyzers produce 1Nm 3 The power consumption of H2 is usually greater than 4kWh. In addition, the added value of the anode product oxygen is not high, and it is easy to mix with hydrogen, resulting in the risk of explosion.
[0004] Therefore, how to further optimize the process of hydrogen production by electrolysis and reduce the overall energy consumption of hydrogen production equipment is an urgent problem to be solved. Summary of the invention
[0005] The technical problem to be solved by the present invention is to overcome the deficiencies in the prior art and provide a method for producing hydrogen by bipolar oxidation of furfural by acid-base asymmetric coupling.
[0006] To solve the technical problem, the solution of the present invention is:
[0007] A method for producing hydrogen by bipolar oxidation of furfural by acid-base asymmetric coupling is provided, comprising the following steps:
[0008] (1) constructing a bipolar hydrogen production system: comprising an anode reaction chamber and a cathode reaction chamber separated by a bipolar membrane or a proton membrane, wherein an anode electrode and a cathode electrode are respectively arranged in the two reaction chambers and connected to a DC power supply through a wire; a mixed solution containing furfural and alkali is filled in the anode reaction chamber as an anode electrolyte, and an acid solution is filled in the cathode reaction chamber as a cathode electrolyte;
[0009] (2) A voltage of 0.35 to 0.50 V is applied to the anode and cathode using a DC power supply; in the anode reaction chamber, furfural is deoxidized to generate furoic acid, and hydrogen is generated through the Tafel reaction; in the cathode reaction chamber, HER hydrogen evolution reaction occurs to generate hydrogen.
[0010] As a preferred embodiment of the present invention, Ar gas is introduced into the anode electrolyte for 10 minutes before the hydrogen production reaction.
[0011] As a preferred embodiment of the present invention, the anolyte is a mixed solution containing furfural and KOH, wherein the concentration of KOH is 1M and the concentration of furfural is 0.3M.
[0012] As a preferred embodiment of the present invention, the cathode electrolyte is a 0.5M H2SO4 solution.
[0013] As a preferred embodiment of the present invention, the inner material of the cathode electrode is nickel foam, titanium foam, titanium felt or carbon paper, and has a Pt / C catalyst or a Ru / NC catalyst on its surface.
[0014] As a preferred embodiment of the present invention, the inner material of the anode electrode is copper foam, and a nano copper-based catalyst is provided on its surface; the anode electrode is prepared by the following method:
[0015] (6.1) Cut copper foam of appropriate size, and ultrasonically clean it with acetone, dilute hydrochloric acid and ethanol for 5 minutes each, and set aside;
[0016] (6.2) Using 3M NaOH solution as electrochemical oxidation electrolyte, cleaned copper foam as anode, and platinum sheet as cathode, current is applied to oxidize the surface of copper foam, forming a nano-scale copper particle structure on its skeleton surface;
[0017] (6.3) Using 0.5 M Na2SO4 solution as the electrochemical reduction electrolyte, oxidized copper foam as the cathode, and platinum sheet as the anode, current is applied to partially reduce the nanoscale copper particle structure to form a low-valent copper-based catalyst containing Cu(111), Cu(200), and Cu(220) structures.
[0018] As a preferred embodiment of the present invention, in step (6.2), the current loaded on the anode is 60 mA cm -2 , duration is 30 minutes.
[0019] As a preferred embodiment of the present invention, in step (6.3), the current loaded on the cathode is 60 mA cm -2 , duration is 30 minutes.
[0020] The present invention also provides a membrane electrode reactor for bipolar hydrogen production based on acid-base asymmetric coupling furfural oxidation, comprising an anode plate, a nano-copper-based catalyst membrane electrode as an anode, a frame-type seal, a bipolar membrane, a frame-type seal, a Ru / NC catalyst membrane electrode as a cathode, and a cathode plate arranged in sequence; the above sheet structures are tightly fitted to form an anode reaction chamber and a cathode reaction chamber separated by the bipolar membrane; the anode and the cathode are respectively connected to a DC power supply through wires; electrolyte inlets and outlets are provided on the anode plate and the cathode plate, and are respectively connected to the corresponding reaction chambers; the membrane electrode reactor also includes two sets of electrolyte circulation systems, each including an electrolyte storage tank, a peristaltic pump and a reaction chamber connected by pipelines, and the electrolyte in the two reaction chambers is kept in self-circulation by the peristaltic pump; wherein the anode electrolyte is a mixed solution of furfural and alkali solution, and the cathode electrolyte is an acid solution; the hydrogen generated by the reaction is carried by the electrolyte to the electrolyte storage tank and discharged from the outlet provided on the tank top.
[0021] As a preferred embodiment of the present invention, the material of the anode plate is stainless steel or nickel, and the material of the cathode plate is titanium, stainless steel plated with titanium, or nickel plated with titanium.
[0022] Description of the invention principle:
[0023] The innovation of the present invention is that the anode oxygen evolution reaction is replaced by an organic small molecule oxidation reaction that is more easily reacted in thermodynamics to achieve a lower starting potential, thereby achieving the purpose of reducing power consumption. In addition, the small molecule oxidation-assisted hydrogen production technology can also achieve the coordinated production of high value-added chemicals. Specifically, the present invention can achieve furfural dehydrogenation oxidation to generate furoic acid in a low voltage range by utilizing the furfural oxidation (FOR) reaction with thermodynamic advantages, and generate hydrogen at the anode through the Tafel reaction. The use of furfural oxidation reaction to replace the oxygen evolution reaction can greatly reduce the reaction energy barrier of electrolytic hydrogen production, and furfural can be prepared into high value-added furoic acid. Among them, the theoretical voltage of furfural oxidation reaction is low (> 0.05V), and the product furoic acid is a precursor of drug molecules and perfumes. Since the conversion process of furoic acid is accompanied by the generation of hydrogen, the coupling of furfural oxidation can achieve bipolar hydrogen production, which further reduces the energy consumption of hydrogen production.
[0024] The invention prepares the nano copper-grade catalyst through electrochemical oxidation and reduction reaction, prepares 2+ nano copper structure through oxidation, reduces 2+ copper through reduction reaction to prepare 0 / 1+ copper active sites, and realizes high current furfural oxidation.
[0025] The present invention utilizes the electrochemical neutralization energy in the acid-base asymmetric reaction system to further reduce the reaction potential difference of hydrogen production by electrolysis.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] 1. The present invention constructs a method for producing hydrogen by bipolar oxidation of furfural by coupling acid-base imbalance, so as to achieve simultaneous hydrogen evolution at the cathode and anode during electrolysis accompanied by the generation of furoic acid, thereby reducing anode energy consumption and achieving high value of biomass energy. In addition, the reaction system does not require a precious metal catalyst, which greatly reduces production costs. The reaction system breaks the limitations of traditional alkaline hydrogen production / proton membrane hydrogen production, and realizes biomass refining while reducing hydrogen production energy consumption and production costs.
[0028] 2. In the present invention, at 0.35V vs. RHE, more than 500mA cm -2 Given a cell voltage of 0.35 V for the membrane electrode, a response current of 120 mA cm -2 The current density is 100%, and the Faraday efficiency of hydrogen production reaches 160%. Compared with the catalyst projects in the existing technology, the furfural oxidation performance is more excellent, with greater economic value and market application prospects;
[0029] 3. The present invention adopts an acid-base asymmetric system, combines anode furfural oxidation, utilizes electrochemical neutralization energy and the thermodynamic advantages of furfural, effectively reduces the voltage of hydrogen production by electrolysis, and greatly reduces the energy consumption of hydrogen production by electrolysis.
[0030] 4. To further improve efficiency, the copper nanocatalyst used in the present invention is prepared by an electrochemical redox method, which is simple and easy to prepare; the nanostructure and oxidation state can be regulated by the current density and time, and the copper raw material reserves are abundant and the cost is low, which is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 Schematic diagram of preparing copper nanocatalyst by electrochemical oxidation-reduction in the present invention;
[0032] Figure 2 This is a SEM morphology structure diagram of the copper catalyst prepared in Example 1 of the present invention;
[0033] Figure 3 The XRD spectrum of the copper catalyst prepared in Example 1 of the present invention;
[0034] Figure 4 Schematic diagram of a three-electrode H-type electrolyzer used to test electrochemical furfural oxidation;
[0035] Figure 5 It is the LSV performance diagram of the copper-based furfural oxidation catalyst prepared in the present invention;
[0036] Figure 6 The schematic diagram of the bipolar hydrogen production system of the acid-base asymmetric furfural oxidation in the present invention;
[0037] Figure 7 It is a diagram of an H-type test device of the present invention;
[0038] Figure 8 The current density comparison under different voltage conditions of the present invention;
[0039] Fig. 9 It is a schematic structural diagram of a membrane electrode reactor for bipolar hydrogen production in the present invention;
[0040] Fig.10 The figure is a comparison of the current density of the membrane electrode under different voltage conditions in the present invention. DETAILED DESCRIPTION
[0041] The present invention is described in detail below with reference to specific embodiments, but the protection scope of the present invention is not limited to these embodiments.
[0042] 1. Embodiment 1 of the present invention
[0043] The copper foam electrode used as an anode has a nano-copper-based catalyst on its surface, and the preparation method comprises the following steps:
[0044] (1) Cut a 1 cm × 2 cm sheet of copper foam and ultrasonically clean it with acetone, dilute hydrochloric acid, and ethanol for 5 minutes each, and set aside;
[0045] (2) Prepare 3M NaOH solution and take 50 mL as electrochemical oxidation electrolyte. Use the copper foam cleaned in step (1) as the anode and the platinum sheet as the cathode (such as Figure 1 a). Load 60 mA cm -2 The anodic current was applied for 30 minutes to oxidize the surface of the copper foam and form a nano-scale copper particle structure on the surface of the skeleton;
[0046] (3) Prepare 0.5M Na2SO4 solution and take 50mL as electrochemical reduction electrolyte. Use the copper foam oxidized in step (2) as cathode and platinum sheet as anode (such as Figure 1 b). Load 60 mA cm -2 The anodic current was applied for 30 minutes to partially reduce the nano-scale copper particle structure on the surface of the copper foam to form a low-valent copper-based catalyst containing Cu(111), Cu(200) and Cu(220) structures.
[0047] When preparing copper-based nanocatalysts in the above manner, it is only necessary to adjust the current density and treatment time in steps (2) and (3) respectively to achieve regulation of the nanostructure and oxidation state of the catalyst to adapt to anode electrolytes with different compatibility relationships.
[0048] 2. Characterize the copper-based nano FOR catalyst prepared in Example 1;
[0049] Morphology analysis: The copper foam with copper-based nanocatalyst on the surface was taken and its microscopic morphology was observed by scanning electron microscopy (SEM). Figure 2 As shown. Figure 2 As can be seen in the right picture, many nanoparticles grow on the surface of copper foam after electrochemical redox treatment. Since nanoparticles have a large specific surface area, more active sites are exposed, which can improve the rate and efficiency of catalytic reactions.
[0050] Structural analysis: Take copper foam with copper-based nanocatalyst on the surface and observe its composition through X-ray diffraction (XRD). The results are as follows: Figure 3 As shown. Figure 3 The copper nanostructure mainly includes Cu(111), Cu(200) and Cu(220) crystal planes, and different copper nanocrystal planes can synergistically catalyze electrochemical reactions.
[0051] 3. Furfural oxidation performance test of the copper foam electrode in Example 1:
[0052] Hg / HgO, the prepared copper foam electrode, and the graphite rod electrode were used as the reference electrode, working electrode, and counter electrode, respectively. Figure 4 The H-type trough three-electrode system shown is used to test the furfural oxidation performance. The H-type trough is separated by a bipolar membrane in the middle, with 1M KOH + 0.3M furfural as the electrolyte on the left and 1M KOH as the electrolyte on the right. Ar gas was introduced into the anode electrolyte for 10 minutes before the test, and Ar gas was continuously introduced during the test.
[0053] The copper foam electrode prepared in Example 1 was subjected to a linear sweep voltammetry (LSV) test in a test range of 0 to 0.8 V vs. RHE and a sweep rate of 10 mV s -1 , the overpotential is 0 V and 10 mA cm relative to the reversible hydrogen electrode -2 The potential difference is measured.
[0054] In order to make the test results more comparable and reliable, the potential is converted from relative to the Hg / HgO electrode to relative to the standard hydrogen electrode (RHE). The conversion relationship is:
[0055] E RHE =E Hg / HgO +0.098+0.0591*pH, pH=14.
[0056] Comparative Example 1
[0057] Untreated original copper foam was used, which was marked as Cu FM. Then, the same operation was performed according to the test steps in the above H-type cell three-electrode system.
[0058] Comparative Example 2
[0059] Referring to the operation of steps (1) and (2) in Example 1, only the cleaned copper foam was heated to 60 mA cm -2 The oxidation treatment is carried out by the oxidation current of 10000, but the reduction treatment is not carried out, which is marked as Cu(OH)2. Then the same operation is carried out according to the test steps in the above H-type cell three-electrode system.
[0060] 4. Comparative experiment and result analysis:
[0061] The hydrogen evolution and furfural oxidation performance tests were carried out as follows:
[0062] (1) The copper foams prepared in Example 1 and the two comparative examples 1 and 2 were used as working electrodes, respectively, and three-electrode systems were constructed in each H-type electrolytic cell.
[0063] (2) The furfural oxidation performance test was carried out on the three-electrode system constructed using three types of copper foams. In the test, the Hg / HgO electrode was converted to a standard hydrogen electrode (RHE), and the conversion relationship was:
[0064] E RHE =E HgO / Hg +0.0591*13.8
[0065] The voltage test range of furfural oxidation (FOR) is 0V~0.4V vs.RHE. The LSV scanning speed is set to 10mVs -1 .
[0066] Figure 5 The LSV curves of copper foams with different implementations are compared. It can be seen from the figure that the response currents of Example 1 (surface copper nanocatalyst, CuNP), Comparative Example 1 (original copper foam, Cu FM) and Comparative Example 2 (oxidized copper foam, Cu(OH)2) are different. Compared with the two comparative examples, the formation of Cu(OH)2 nanoparticles after oxidation is conducive to exposing more specific surface area, and then the Cu 2+ Reduction to Cu + / Cu 0 The copper foam electrode of Example 1 (CuNP) has a larger response current because it has not been oxidized. Therefore, no nanoparticles are generated in Comparative Example 1, resulting in a relatively small response current. 2+ Therefore, a negative current is shown in the 0-0.1V scanning interval, indicating that a large amount of Cu 2+ In the restoration phase.
[0067] 5. H-type tank acid-base asymmetric bipolar hydrogen production performance test
[0068] 5.1 Technical principle:
[0069] i. The working principle of acid-base asymmetric bipolar hydrogen production is as follows Figure 6 As shown, according to Gibbs free energy:
[0070] ΔG cell =-nF(E θ +0.0591*ΔpH)
[0071] When ΔpH=14, a voltage of 0.83V can be generated, which is the electrochemical neutralization energy, reducing the pressure of the electrolytic hydrogen production cell.
[0072] ii. Principle of Furfural Oxidation and Hydrogen Evolution:
[0073] 2R-CHO+OH - =R-COO - +2H2O+2e - +H2
[0074] In addition, adding furfural, which has thermodynamic advantages, to the anode to replace the traditional OER reaction will further reduce the cell pressure of hydrogen electrolysis. In the lower oxidation potential range, the H on the two CHO will couple to generate one H2 after undergoing the Tafel process.
[0075] 5.2 System Construction:
[0076] The bipolar hydrogen production system includes an anode reaction chamber and a cathode reaction chamber separated by a bipolar membrane (or proton membrane); an anode electrode and a cathode electrode are respectively arranged in the two reaction chambers and connected to a DC power supply through wires; a mixed solution containing furfural and alkali is filled in the anode reaction chamber as an anode electrolyte, and an acid solution is filled in the cathode reaction chamber as a cathode electrolyte.
[0077] In this example, Ru / NC is used as the cathode hydrogen evolution electrode, the internal material of which is nickel foam, titanium foam, titanium felt or carbon paper, and the surface of which has a Ru / NC catalyst. The preparation method and attachment method of the Ru / NC catalyst can be referred to Yang Li et al. Carbon 183 (2021) 362-367. Pt / C catalyst can also be used instead, and its preparation method and attachment method can be referred to Yang Li et al. Carbon 183 (2021) 362-367.
[0078] For example, the bipolar membrane may be a commercial product of Cree.
[0079] 5.3 Test conditions:
[0080] like Figure 7As shown, Ru / NC is used as the cathode hydrogen evolution electrode, and the copper foam electrode prepared in Example 1 is used as the anode electrode; the cathode electrolyte is a 0.5M H2SO4 solution, and the anolyte is a mixed solution of 1M KOH+0.3M furfural, separated by a bipolar membrane. Ar gas was introduced into the anolyte for 10 minutes before the test, and Ar gas was continuously introduced during the test. Chenhua CHI1140C electrochemical workstation was used to give different electrolytic cell voltages. The response current density of 0.35V, 0.4V, and 0.5V was tested.
[0081] In addition, in order to compare with the acid-base asymmetric system, a reaction system in which the cathode and anode electrolytes are both 1.0M KOH is used as a comparison. Figure 8 As shown in the figure, the electrolysis current of the pure alkaline system is less than 35 mA cm at the three potentials of 0.35 V, 0.40 V and 0.50 V. -2 In the acid-base asymmetric system exemplified in the present invention, the response current is greater than 65 mA cm at different electrolysis voltages. -2 , thus showing the advantages of the acid-base asymmetric system.
[0082] 6. Acid-base asymmetric bipolar hydrogen production performance test of membrane electrode reactor
[0083] In order to further optimize the reactor structure and reduce the resistance in the cell, this example uses a membrane electrode to build a membrane electrode reactor and conducts a bipolar hydrogen production test.
[0084] like Fig. 9 As shown, the membrane electrode reactor includes an anode plate, a nano-copper-based catalyst membrane electrode as an anode, a frame-type seal, a bipolar membrane, a frame-type seal, a Ru / NC catalyst membrane electrode as a cathode, and a cathode plate arranged in sequence; the above sheet structures are tightly fitted to form an anode reaction chamber and a cathode reaction chamber separated by a bipolar membrane; the anode and the cathode are respectively connected to a DC power supply through wires; an electrolyte inlet and outlet are provided on the anode plate and the cathode plate, and are respectively connected to their corresponding reaction chambers. The preparation method of the nano-copper-based catalyst membrane electrode of the anode refers to the steps of Example 1, and the preparation method of the Ru / NC catalyst membrane electrode refers to the records of Yang Li et al. Carbon 183 (2021) 362-367. The inner materials of the two electrodes are pre-cut (or pressed) into thin sheet materials and then the catalyst is attached.
[0085] The membrane electrode reactor also includes two sets of electrolyte circulation systems, each of which includes an electrolyte storage tank, a peristaltic pump (not shown in the figure) and a reaction chamber connected by pipelines. The peristaltic pump is used to keep the electrolytes in the two reaction chambers in self-circulation; wherein the anode electrolyte is a mixed solution of furfural and alkali solution, and the cathode electrolyte is an acid solution; the hydrogen generated by the reaction is carried by the electrolyte to the electrolyte storage tank and discharged from the outlet provided on the top of the tank.
[0086] As an example, the cathode electrolyte is 0.5M H2SO4 solution, and the anode electrolyte is 1M KOH + 0.3M furfural mixed solution. Chenhua CHI1140C electrochemical workstation is used to set different electrolytic cell voltages. The response current density of 0.35V, 0.40V, and 0.50V is tested. The test results are as follows Fig.10 As shown, the current density is greater than 100 mA cm -2 , the test current density is twice that of the H-type slot test result.
[0087] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for producing hydrogen by bipolar oxidation of furfural by acid-base asymmetric coupling, characterized in that: The following steps are involved: (1) Constructing a bipolar hydrogen production system: comprising an anode reaction chamber and a cathode reaction chamber separated by a bipolar membrane, wherein an anode electrode and a cathode electrode are respectively arranged in the two reaction chambers and connected to a DC power supply through a wire; the anode reaction chamber and the cathode reaction chamber are respectively filled with an anolyte and a cathode electrolyte; the anolyte is a mixed solution containing furfural and KOH, wherein the concentration of KOH is 1 M and the concentration of furfural is 0.3 M; the cathode electrolyte is a 0.5 M H2SO4 solution; The anode electrode is prepared by the following method: (a) Cut copper foam of appropriate size, clean it with acetone, dilute hydrochloric acid and ethanol ultrasonically for 5 minutes each, and set aside; (b) Using 3M NaOH solution as the electrochemical oxidation electrolyte, the cleaned copper foam as the anode, and the platinum sheet as the cathode, current is applied to oxidize the surface of the copper foam, forming a nano-scale copper particle structure on its skeleton surface; (c) Using 0.5 M Na2SO4 solution as the electrochemical reduction electrolyte, the oxidized copper foam as the cathode, and the platinum sheet as the anode; applying current to partially reduce the nanoscale copper particle structure to form a low-valent copper-based catalyst containing Cu(111), Cu(200), and Cu(220) structures; (2) Before the hydrogen production reaction, Ar gas was introduced into the anode electrolyte for 10 minutes, and then a voltage of 0.35-0.50 V was applied to the anode and cathode using a DC power supply. In the anode reaction chamber, furfural was deoxidized to produce furoic acid, and hydrogen was generated through the Tafel reaction. In the cathode reaction chamber, HER hydrogen evolution reaction occurred to generate hydrogen.
2. The method according to claim 1, characterized in that The cathode electrode is made of nickel foam, titanium foam, titanium felt or carbon paper, and has a Pt / C catalyst or a Ru / NC catalyst on its surface.
3. The method according to claim 1, characterized in that In step (b), the current loaded on the anode is 60 mA cm -2 , duration is 30 minutes.
4. The method according to claim 1, characterized in that: In step (c), the current loaded on the cathode is 60 mA cm -2 , duration is 30 minutes.