A photochromic copper-doped KTN single crystal, preparation method and application

Cu-KTN crystals were prepared by straight-pull single crystal method, and Cu ion doping was used to improve the electro-optical performance and photochromic properties of KTN crystals, which solved the problem of insufficient deflection angle and photochromic effect of KTN crystals, and achieved large deflection angle and high efficiency Photochromicity promotes the application of electro-optical functional materials.

CN117265661BActive Publication Date: 2024-11-26NEW MATERIAL INST OF SHANDONG ACADEMY OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311243440.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-22
Publication Date
2024-11-26
Estimated Expiration
2043-09-22

AI Technical Summary

Technical Problem

In the prior art, the beam deflection angle of KTN crystals is less studied, especially the electro-optical effect of ion-doped KTN single crystals is insufficient, and there are no related reports on the photochromic effect of KTN crystals, which limits the optical signal acquisition and spatial targets. Ability to change posture.

Method used

Copper-doped KTN (Cu-KTN) crystals were prepared by direct pulling single crystal manufacturing method. Cu ion doping was used to improve the electro-optical performance and photochromic properties of the crystals, so that they appeared red-brown, green or red under 405nm ultraviolet light irradiation. The light is light green and reversibly recovers, increasing the beam deflection angle under the applied voltage.

Benefits of technology

It realizes the efficient photochromicity and large deflection angle of Cu-KTN crystal, improves the beam deflection performance, provides a new way to improve photocurrent for photoexcited carriers, promotes the application of electro-optical functional materials, and is suitable for photochromic and beam deflection devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117265661B_ABST
    Figure CN117265661B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of bulk single crystal processing, and specifically relates to a photochromic copper-doped KTN single crystal, a preparation method and its application. The present invention prepares Cu-KTN crystals by a Czochralski single crystal manufacturing method, and for the first time finds that Cu-KTN crystals exhibit different colors, and the process can be reversibly controlled. In addition, Cu-doped KTN increases the photocurrent under an applied voltage, so that the beam deflection angle increases when irradiated with 405nm light. The present invention explores Cu-doped KTN single crystals, which have great value for new photochromic materials on the one hand, and for photoexcited carriers on the other hand to improve the size of the photocurrent, increase the beam deflection angle, and promote the application of electro-optical functional materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of bulk single crystal processing, and in particular relates to a photochromic copper-doped KTN single crystal, a preparation method and an application thereof. Background Art

[0002] Satellite laser communication in space communication has the advantages of strong confidentiality and large capacity. As an important way to achieve confidential communications between satellites and the ground, between satellites, and between space and ground, it has become a research hotspot for space communications in various countries. In order to realize the collection and networking of multiple sets of optical signals, it is necessary to change the working direction of the transmitter and receiver. However, due to the limitations of orbits and energy, space targets and spacecraft cannot change their posture and position at will. As an important device, the beam deflector can regularly change the propagation direction of the beam, which can solve this problem well in space. Beam deflection technology is also widely used in optical storage, imaging, laser scanning and other fields, and can be divided into two categories: mechanical and non-mechanical. Mechanical beam deflection technology usually uses galvanometers, rotating mirrors, or micro-electromechanical scanning mirrors. Due to the inertia of mechanical components, the stability and scanning frequency are easily low, and a larger deflection angle requires a combination of multiple prisms. Therefore, the complexity of device design is not suitable for the development of miniaturized electronic devices. Researchers have successively carried out in-depth exploration of non-mechanical deflection technologies such as acousto-optic deflection technology, liquid crystal deflection technology, and electro-optical deflection technology. In particular, electro-optic deflection devices have the advantages of small size, fast response speed, and better ability to meet the needs of high-frequency scanning. The electro-optic deflector utilizes the electro-optic effect, that is, the refractive index of the crystal changes under the action of an external voltage, thereby changing the propagation direction of the light beam. Research on electro-optic effect deflection devices generally focuses on uniaxial crystals with piezoelectric effect, using their linear electro-optic effect to achieve light beam deflection. In the past, the secondary electro-optic effect of crystal materials was rarely used. This is because the secondary electro-optic effect of general crystals is much smaller than the linear electro-optic effect, making it difficult to apply. In recent years, a series of excellent secondary electro-optic crystal materials such as BaTiO3, SrTiO3, and Sr have been reported at home and abroad. x Ba 1-x Nb2O6. It can not only control the direction of light beam propagation, but also has much better performance in response speed, deflection voltage, etc. than the currently widely used linear electro-optical crystal materials, the most representative of which is potassium tantalate niobate (KTN) crystal.

[0003] KTN crystal is a solid solution mixed crystal of potassium tantalate and potassium niobate. The phase structure (cubic phase, tetragonal phase or orthorhombic phase) of the crystal is controlled by controlling the ratio of Ta and Nb occupying the B position. The dielectric constant at the interface between the tetragonal phase and the cubic phase is the largest, showing a huge Kerr effect. In order to improve the performance, a series of methods to improve the performance of crystals have been proposed, and the most representative one is ion doping. E.DelRe et al. studied KTN:Li crystals and found that KTN:Li showed a strong electromechanical coupling. In the non-equilibrium state, the thermal history of the crystal can be used to realize the scale-free propagation of light in the crystal, proving the great potential of KTN crystals in the field of super-resolution. D.Pierangeli et al. discovered a series of novel optical phenomena such as optical solitons and optical superlattices in KTN:Li crystals. This discovery provides an important reference for the research and development of related optical devices such as optical structure memory, spatial resolution satellites and electro-optical devices. Xilong Cao et al. found that the defect dipoles introduced by Fe ions in KTN:Fe can affect the reorientation of domain structure. Ferroelectricity and piezoelectricity are related to the content of doped Fe ions, proving that doping can adjust the performance of ABO3 perovskite. Yu Wang et al. found that Mn-doped KTN introduced strong local heterogeneity, which reduced the size of the domain structure, weakened the dipole correlation, and enhanced the piezoelectric properties, which is of great value for optimizing material properties.

[0004] In summary, in order to realize the optical signal collection of space laser communication and to change the attitude and position of space targets and spacecraft at will, it is urgent to improve the deflection performance of the beam deflector. However, there are still few studies on the electro-optical effect of ion-doped KTN single crystals, especially on how to improve the beam deflection angle of KTN crystals.

[0005] In addition, photochromism has been widely used, but there are no relevant reports on the photochromic effect of KTN crystals. There is still a lot of room for research on the application expansion of electro-optical functional materials. Summary of the invention

[0006] In view of the above-mentioned deficiencies of the prior art, the present invention prepares Cu-KTN crystals by a Czochralski single crystal manufacturing method. It is found for the first time that Cu-KTN crystals exhibit different colors, and the process can be reversibly controlled. At the same time, Cu-doped KTN increases the photocurrent under applied voltage, so that the beam deflection angle increases when irradiated with 405nm light.

[0007] In one aspect, the present invention provides a photochromic copper-doped KTN single crystal, wherein the molecular formula of the KTN single crystal is M:KTa 1-x Nb xO3; M is Cu or a combination of Cu and other elements, preferably Cu or a combination of Cu and other metal elements, more preferably Cu or a combination of Cu and Fe; 0<x<1, the doping ion concentration ratio of Cu is>0;

[0008] When M is Cu, when the single crystal is irradiated with ultraviolet light of 405nm or less, the color changes from yellow-green to reddish brown, and after the irradiation is stopped, the color gradually returns to yellow-green; when irradiated with green light or long-wavelength light, the color changes to light green, and after the irradiation is stopped, the color gradually returns to yellow-green.

[0009] Further improvement of this scheme, each mol of M:KTa 1-x Nb x The sum of the molar numbers of O3, K, Cu and Fe is 1. Preferably, the ratio of each element is Cu:K:Ta:Nb:O=0.01:0.99:0.595:0.405:3.

[0010] In another aspect, the present invention provides a method for preparing a photochromic copper-doped KTN single crystal, comprising the following steps:

[0011] (1) KTa doped with Cu or Cu and Fe as required 1-x Nb x The ratio of O3, Ta2O5, Nb2O5, K2CO3, CuO / Cu2O / Cu / Fe2O3 raw materials are configured, and after being mixed and stirred evenly, they are placed in a furnace for pre-sintering; the crucible containing the pre-sintered product is placed in the center of the temperature field of the crystal growth furnace; the temperature amplitude, pulling speed and growth temperature are controlled by the pulling method;

[0012] (3) After 7-10 days of crystal growth, the temperature is lowered to room temperature to obtain a Cu-KTN or Cu-Fe-KTN single crystal.

[0013] In a further improvement of this scheme, the molar ratio of Ta2O5 and Nb2O5 in step (1) is 1-x:x.

[0014] In a further improvement of the present invention, the pre-sintering temperature of step (1) is 800-1000°C.

[0015] In a further improvement of the present scheme, the temperature range of step (1) is 0.2-1°C.

[0016] In a further improvement of the present invention, the pulling speed of step (1) is 0.01 mm / h-2 mm / h, and the growth temperature of step (1) is 1000-1500° C. Inappropriate temperature may cause defects, bubbles, opacity, and cracking in the crystal.

[0017] A further improvement of this scheme is that the CuO or Cu or Cu2O in step (1) is M:KTa per mol 1-x Nb x The molar amount of Cu in O3 is added in a ratio of 0.001% to 20%.

[0018] A more preferred method for preparing a photochromic copper-doped KTN single crystal comprises the following steps:

[0019] (1) The configuration components are Cu:KTa 0.6 Nb 0.4 The amount of O3 raw materials, the molar ratio of CuO, K2CO3, Ta2O5, and Nb2O5 is 0.01:0.495:0.3:0.2. After being mixed and stirred evenly, they are placed in a muffle furnace at 900°C for pre-sintering for 12 hours; the platinum crucible containing the pre-sintered product is placed in the center of the temperature field of the crystal growth furnace, and the temperature amplitude is accurately controlled at 0.2°C by the pulling method, the pulling speed is controlled at 0.3mm / h, and the growth temperature is 1300°C;

[0020] (2) After the crystal growth is completed in one week, the temperature is cooled to room temperature to obtain a large Cu-KTN single crystal;

[0021] (3) Orient, cut, and polish the crystal into Cu-KTN crystals of a certain size for later use.

[0022] In addition, the present invention provides application of the photochromic copper-doped KTN single crystal in the field of photochromism or the field of increasing the deflection angle of a light beam.

[0023] The beneficial effects of the present invention are:

[0024] (1) The present invention prepares Cu-KTN crystals by a Czochralski single crystal manufacturing method, thereby improving the electro-optical properties of the crystals. It is first discovered that Cu-KTN crystals exhibit different colors under different wavelengths of light, reddish brown after 405nm ultraviolet light irradiation, light green after green or red light irradiation, and gradually recover after the light irradiation stops, and the process can be reversibly controlled. This photochromic phenomenon is attributed to the change in valence of copper ions, and light irradiation promotes the generation of electrons and holes.

[0025] (2) Cu-doped KTN increases the photocurrent under applied voltage, which increases the beam deflection angle when irradiated with 405nm light. The deflection angle of Cu-KTN (18.6mrad, 1400V) crystal is larger than that of pure KTN (14.82mrad, 1400V) crystal. Moreover, the beam deflection angle increases with the increase of optical power, which provides a new approach for beam deflectors with large deflection angles.

[0026] (3) The present invention explores Cu-doped KTN single crystals, which have great value for novel photochromic materials on the one hand and for improving the size of photocurrent of photoexcited carriers on the other hand, and promoting the application of electro-optical functional materials. Cu-doped KTN single crystals can accelerate the application in light deflection and space optical communication. In addition, the Cu-doped KTN crystals of the present invention can also be used in crystal modulation, which is conducive to the realization of the strategy of photochromic high-functional single crystal optical devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0028] Figure 1 (a) XRD refined spectra of KTN and Cu-KTN, (b) dielectric constants of KTN and Cu-KTN crystals at different temperatures, (c) (d) the variation of ln(1 / εr-1 / εmax) with ln(T-Tc) of KTN (c) crystal (c) and Cu-KTN crystal (d), the solid line is the fitting curve γ of (c) (d);

[0029] Figure 2 (a) 6×6×3KTN supercell, (b) KTN-1%Cu supercell;

[0030] Figure 3 (ab) are pure KTN crystals, (cd) are Cu-KTN crystals in a naturally placed state, (e) Cu-KTN crystals after 405nm light irradiation for 10s, (f) Cu-KTN crystals after 405nm light irradiation for 60s, (g) Cu-KTN crystals after green light irradiation;

[0031] Figure 4 (a) and (b) are the IV curves of KTN (a) and Cu-KTN (b) at different wavelengths of optical power. (c) and (d) are the IV curves of KTN (c) and Cu-KTN (d) at a wavelength of 405 nm.

[0032] Figure 5 (a) is the UV-visible absorption spectra of KTN and Cu-KTN, (b) is the UV-visible absorption spectra of Cu-KTN (αhν) 2 The relationship between hν, (c) is the high-resolution cu2p spectrum of Cu-KTN, and (d) is the EPR of KTN and Cu-KTN;

[0033] Figure 6 KTN(αhν) 2Relationship with hν;

[0034] Figure 7 (a) is the Cu k-edge XANES spectrum, (b) is the Fourier transform of EXAFS data in r space of Cu-KTN and reference sample, (c) is the wavelet change of Cu K-edge in Cu-KTN, (d) is the a-space result obtained by EXAFS fitting of Cu K-edge;

[0035] Figure 8 (a) is the beam deflection angle under different voltage control without irradiation, and (b) is the beam deflection angle under the same voltage under different 405nm light irradiation. DETAILED DESCRIPTION

[0036] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0037] Example 1

[0038] (1) Configuration component is KTa 0.6 Nb 0.4 The amount of O3 raw materials, CuO, K2CO3, Ta2O5, Nb2O5 molar ratio is 0.01:0.495:0.3:0.2, after being mixed and stirred evenly, it is placed in a muffle furnace at 900℃ for pre-sintering for 12h. The platinum crucible containing the pre-sintered product is placed in the center of the temperature field of the crystal growth furnace. The temperature amplitude is accurately controlled at 0.2℃ by the pulling method, the pulling speed is controlled at about 0.3mm / h, and the growth temperature is 1300℃.

[0039] (2) After the crystal growth is completed in one week, the temperature is lowered to room temperature to obtain a large Cu-KTN single crystal. The crystal is oriented, cut, and polished into a Cu-KTN crystal of a certain size for later use.

[0040] Example 2

[0041] (1) Configuration component is KTa 0.6 Nb 0.4The amount of O3 raw materials, Cu2O, K2CO3, Ta2O5, Nb2O5 molar ratio is 0.01:0.99:0.6:0.4, after being mixed and stirred evenly, it is placed in a muffle furnace at 900℃ for pre-sintering for 12h. The platinum crucible containing the pre-sintered product is placed in the center of the temperature field of the crystal growth furnace. The temperature amplitude is accurately controlled at 0.2℃ by the pulling method, the pulling speed is controlled at about 0.3mm / h, and the growth temperature is 1300℃.

[0042] (2) After the crystal growth is completed in about a week, the temperature is cooled to room temperature to obtain a large Cu-KTN single crystal. In actual operation, K2CO3 can be slightly excessive to ensure the normal reaction.

[0043] Example 3

[0044] (1) Configuration component is KTa 0.6 Nb 0.4 The amount of O3 raw materials, the molar ratio of Cu, K2CO3, Ta2O5, and Nb2O5 is 0.01:0.495:0.3:0.2. After being mixed and stirred evenly, they are placed in a muffle furnace at 900°C for pre-sintering for 12 hours. The platinum crucible containing the pre-sintered product is placed in the center of the temperature field of the crystal growth furnace. The temperature amplitude is accurately controlled at 0.2°C by the pulling method, the pulling speed is controlled at about 0.3mm / h, and the growth temperature is 1300°C.

[0045] (2) After the crystal growth is completed in about a week, the temperature is cooled to room temperature to obtain a large Cu-KTN single crystal.

[0046] Example 4

[0047] (1) Configuration component is KTa 0.1 Nb 0.9 The amount of O3 raw materials, CuO, K2CO3, Ta2O5, Nb2O5 molar ratio is 0.01:0.495:0.05:0.45. After mixing and stirring evenly, it is placed in a muffle furnace at 800℃ for pre-sintering for 12h. The platinum crucible containing the pre-sintered product is placed in the center of the temperature field of the crystal growth furnace. The temperature amplitude is accurately controlled at 0.2℃ by the pulling method, the pulling speed is controlled at about 0.01mm / h, and the growth temperature is 1000℃.

[0048] (2) After the crystal growth is completed in about a week, the temperature is cooled to room temperature to obtain a large Cu-KTN single crystal.

[0049] Example 5

[0050] (1) Configuration component is KTa 0.9 Nb 0.1The amount of O3 raw materials, the molar ratio of Cu0, K2CO3, Ta2O5, and Nb2O5 is 0.01:0.495:0.45:0.05.

[0051] After mixing and stirring evenly, it is placed in a muffle furnace at 900℃ for pre-sintering for 12 hours. The platinum crucible containing the pre-sintered product is placed in the center of the temperature field of the crystal growth furnace. The temperature amplitude is precisely controlled at 0.2℃ by the pulling method, the pulling speed is controlled at about 0.3mm / h, and the growth temperature is 1350℃.

[0052] (2) After the crystal growth is completed in about a week, the temperature is cooled to room temperature to obtain a large Cu-KTN single crystal.

[0053] Example 6

[0054] (1) Configuration component is KTa 0.6 Nb 0.4 The amount of O3 raw materials, CuO, K2CO3, Ta2O5, Nb2O5 molar ratio is 0.001%: 0.99999: 0.3: 0.2, after being mixed and stirred evenly, it is placed in a muffle furnace at 900℃ for pre-sintering for 12 hours. The platinum crucible containing the pre-sintered product is placed in the center of the temperature field of the crystal growth furnace. The temperature amplitude is accurately controlled at 0.2℃ by the pulling method, the pulling speed is controlled at about 0.2mm / h, and the growth temperature is 1350℃.

[0055] (2) After the crystal growth is completed in about a week, the temperature is cooled to room temperature to obtain a large Cu-KTN single crystal.

[0056] Example 7

[0057] (1) Configuration component is KTa 0.6 Nb 0.4 The amount of O3 raw materials, the molar ratio of CuO, K2CO3, Ta2O5, and Nb2O5 is 0.2:0.4:0.3:0.2.

[0058] After mixing and stirring evenly, it is placed in a muffle furnace at 900℃ for pre-sintering for 12 hours. The platinum crucible containing the pre-sintered product is placed in the center of the temperature field of the crystal growth furnace. The temperature amplitude is precisely controlled at 0.2℃ by the pulling method, the pulling speed is controlled at about 0.2mm / h, and the growth temperature is 1380℃.

[0059] (2) After the crystal growth is completed in about a week, the temperature is cooled to room temperature to obtain a large Cu-KTN single crystal.

[0060] Example 8

[0061] (1) Configuration component is KTa 0.6 Nb 0.4The amount of O3 raw materials, CuO, K2CO3, Ta2O5, Nb2O5 molar ratio is 0.01:0.495:0.3:0.2. After being mixed and stirred evenly, it is placed in a muffle furnace at 1000℃ for pre-sintering for 12 hours. The platinum crucible containing the pre-sintered product is placed in the center of the temperature field of the crystal growth furnace. The temperature amplitude is accurately controlled at 1℃ by the pulling method, the pulling speed is controlled at about 2mm / h, and the growth temperature is 1500℃.

[0062] (2) After the crystal growth is completed in about a week, the temperature is cooled to room temperature to obtain a large Cu-KTN single crystal.

[0063] Comparative Example 1

[0064] (1) Configuration component is KTa 0.6 Nb 0.4 The amount of O3 raw materials, the molar ratio of K2CO3, Ta2O5, and Nb2O5 is 1:0.6:0.4.

[0065] After mixing and stirring evenly, it is placed in a muffle furnace at 900℃ for pre-sintering for 12 hours. The platinum crucible containing the pre-sintered product is placed in the center of the temperature field of the crystal growth furnace. The temperature amplitude is precisely controlled at 0.2℃ by the pulling method, the pulling speed is controlled at about 0.2mm / h, and the growth temperature is 1350℃.

[0066] (2) After the crystal growth is completed in about a week, the temperature is lowered to room temperature to obtain a large KTN single crystal. The crystal is oriented, cut, and polished into KTN crystals of a certain size for later use.

[0067] The X-ray powder diffraction pattern of the KTN crystal prepared in Comparative Example 1 is as follows: Figure 1 (a) As shown in the figure below, the X-ray powder diffraction pattern of the Cu-KTN crystal prepared in Example 1 is as follows Figure 1 (a) As shown in the figure above. The peaks of the X-ray powder diffraction pattern are the characteristic planes of (100), (110), (111), (200), (210) and (211). The diffraction peaks of Cu-KTN and pure KTN are very sharp, indicating that the crystallinity is good. The phase structure of Cu-KTN has not been changed compared with pure KTN, indicating that the Cu element has been successfully incorporated into KTN. Figure 1As shown in b, the temperature dependence of the relative dielectric constant (εr) of KTN and Cu-KTN crystals. The relative dielectric constant is a dimensionless constant. The greater the polarization degree of the dielectric, the greater the dielectric constant. From low temperature to high temperature, εr first increases and then decreases. The temperature corresponding to the peak value is the Curie temperature (Tc). At Tc, the crystal undergoes a phase transition from the ferroelectric phase to the paraelectric phase. The peak value of KTN is εr = 19174.8, Tc = 31.4°C and the peak value of Cu-KTN is εr = 21828.4, Tc = 33.1°C. Calculation shows that the composition of the KTN crystal is KTa 0.597 Nb 0.403 O3, Cu-KTN crystal composition is KTa 0.595 Nb 0.405 O3. The doping amount of Cu element was determined by ICP to be 0.98%. Generally speaking, the higher the proportion of Ta, the lower the Tc and the larger the εr. The Ta content of Cu-KTN is lower than that of KTN, but the εr is higher than that of KTN. In pure KTN crystal, only the eccentric displacement of Nb ions, the orientation movement of dipoles, and the polar nano-regions (PNR) contribute to polarization. Cu ion doping produces additional defect dipoles that increase the polarization strength, so the dielectric constant of Cu-KTN is large. Figure 1 c, 1d are the fitting results of the dielectric temperature spectrum, and its slope is the relaxation factor. Generally speaking, when γ = 1, the material does not have relaxation behavior during phase change, indicating that it is a normal ferroelectric. When γ = 2, the dielectric temperature spectrum peak of the material is diffuse during phase change, which is a typical relaxor ferroelectric. When γ = 1-2, the material is an incomplete diffusion phase change, which is a weak relaxor ferroelectric. The relaxation factor of Cu-KTN (γ = 1.15) is greater than that of KTN (γ = 1.12), and both are weak relaxor ferroelectrics. KTN only has random distribution of Nb and Ta ions at the B position, while Cu-KTN also has random distribution of K and Cu ions at the A position. This disordered distribution of polar micro-regions will cause differences in Curie temperature, making the Cu-KTN phase change peak slightly wider. The dipoles in the polar micro-regions are polarized under the action of the electric field, resulting in Debye dielectric relaxation.

[0068] The 6×6×3 supercell structure of the KTN crystal prepared in Comparative Example 1 is as follows Figure 2 (a) shows that the 6×6×3 supercell structure of the Cu-KTN crystal prepared in Example 1 is as follows Figure 2 (b). Figure 2As shown in the figure, in order to construct a 6×6×3 supercell structure, the number of Nb / Ta atoms is set to 64 / 44, and the arrangement is set to a uniform arrangement of

[111] . Using the first principle calculation from the energy point of view, it is proved that Cu occupies the K metal site of KTN. Because the energy required to replace the K position (1.023eV) is the lowest, and the energy of the final state (-1076.174eV) is the lowest and most stable, it means that Cu doping is most likely to replace the K site. The calculation results are well matched with the XRD fine results and the test results of the dielectric temperature spectrum.

[0069] The photo of KTN crystal prepared in Comparative Example 1 is as follows Figure 3 (a, b) shows the Cu-KTN crystal prepared in Example 1. Figure 3 (cg) In order to study the spatial charge injection effect, electrical conductivity and photochromic properties of KTN crystals, the crystals were irradiated with light of different wavelengths. Figure 3 (ab) shows a colorless and transparent pure KTN crystal. The color of KTN crystal remains unchanged no matter what wavelength light it is irradiated with. Figure 3 As shown in (cd), the Cu-KTN crystal placed at room temperature in the natural state without light irradiation is yellow-green and transparent. Figure 3 (ef) shows that Cu-KTN crystal gradually turns reddish brown under 405nm blue-violet light or ultraviolet light irradiation, and the color gradually deepens with the increase of irradiation time. After about 12 hours of stopping the light, the brown-red color of Cu-KTN can slowly return to yellow-green, and heating can promote this process. Figure 3 As shown in (g), the Cu-KTN crystal turns light green under long-wavelength light irradiation such as green light (535nm) or red light (650nm), and the color gradually becomes lighter as the irradiation time increases. And the photochromic reaction can be repeated reversibly. This phenomenon shows that the Cu-doped KTN single crystal has a controllable, fast and reversible photochromic reaction.

[0070] In addition, the Cu-KTN crystals obtained in Examples 1-8 all achieved photochromic properties, indicating that trace amounts of Cu doping can achieve this effect, providing convenience for large-scale applications.

[0071] The IV curves of the KTN crystal prepared in Comparative Example 1 at different wavelengths and at a wavelength of 405 nm are as follows: Figure 4 As shown in (a, c), the IV curves of the Cu-KTN crystal prepared in Example 1 at different wavelengths and at the optical power of 405 nm are as follows Figure 4 (b, d) In order to describe the effect of photon irradiation on charge density, an electrometer was used to measure the IV curve of the crystal at different wavelengths and powers. Figure 4a, 4b are IV curves under no light, green light, and red light irradiation. It can be seen that as the voltage increases, the current remains almost unchanged. Figure 4 As shown in c and 4d, the IV curve under 405nm blue ultraviolet light is an Ohm curve. As the voltage increases, the current value increases. Because the conductivity of semiconductors is directly related to the carrier concentration, the conductivity can be changed by regulating the carrier concentration. However, most of the electrons in semiconductors are bound by atomic nuclei in covalent bonds and cannot move freely and participate in conduction. When sufficiently strong light irradiates the semiconductor, the immobile electrons in the covalent bonds can be excited to form movable free electrons and participate in conduction, thereby changing the conductivity of the semiconductor. However, light also has strengths, that is, the energy of photons is different. If the photon energy is weak, it may not be possible to excite the electrons, indicating that the energy of green light and red light is less than the bandgap width of KTN, and the energy of 405nm and ultraviolet light is greater than the bandgap width. Only under the effective excitation of 405nm and UV will the current density increase. This shows that the 405nm light excitation reduces the shielding effect, the electrons absorb the energy of this band, the kinetic energy of the electrons increases, and the possibility of electrons escaping from the captured quantum well increases. The reduction of the capture effect increases the mobility of electrons, thereby increasing the injection density and depth of electrons. The free charge density is proportional to the injected current density. As the injected current density increases, photon excitation can increase the free charge density. When the KTN crystal is irradiated by light, the electrons in the valence band receive energy and the electrons break away from the covalent bonds. When the energy of the photon is greater than the bandgap width of the semiconductor, the photon can excite the electrons in the valence band to the conduction band, generating electron and hole pairs, both of which are involved in conduction. For pure KTN, the conductivity generated by light is intrinsic photoconductivity. Light energy can also excite the impurity energy levels in Cu-KTN to generate additional impurity photoconductivity, so the increase in the current of Cu-KTN is greater than that of KTN.

[0072] The UV absorption, EPR, and XPS of the KTN crystal prepared in Comparative Example 1 and the Cu-KTN crystal prepared in Example 1 are as follows: Figure 5 In order to compare the optical band gaps of KTN and Cu-KTN, absorption spectra were tested. Figure 5 In (a), the absorption spectrum of Cu-KTN has two more absorption peaks than that of KTN. The absorption peak at 310nm is attributed to the charge migration of O2+→Cu2+, and the absorption peak at 700nm is due to Cu 2+ The energy level transition between the dd orbitals of 2B1g→2B2g. Figure 6 The band gap of KTN is 3.62 eV. Figure 5 As shown in Fig. 2b, the band gap of Cu-KTN is 3.08 eV. It can be seen that the band gap of Cu-KTN becomes narrower, so that the number of e-h+ pairs under photon excitation increases and the current density increases. Figure 5c is the fitting curve of Cu2p of yellow-green crystal. According to the peak positions of 933.12 and 952.82 eV and the obvious oscillation peak at 940.5 eV, it can be seen that it is Cu2 + .right Figure 3 The XPS spectrum of the light brown-red crystal Cu2p shown in e is fitted, and the binding energy of Cu2p3 / 2 is found to be 932.71 eV, indicating that after 405 nm light irradiation, Cu 2+ Convert to monovalent Cu + .right Figure 3 f, the XPS spectrum of brown-red crystal Cu2p was fitted, and the binding energy of Cu2p3 / 2 was found to be 932.59 eV. As the irradiation time increased, the 2p peak shifted negatively, and the Cu 2+ The oscillation peak disappears. This indicates that the Cu in the yellow-green crystal is mainly Cu 2+ , the Cu in the brown-red crystals is mainly Cu 0 Since the Cu2p peaks of copper ions with different valence states in the XPS test are very close, electron paramagnetic resonance (EPR) test was performed to further clarify the valence state of copper ions. Figure 5 As shown in d, the red curve has no diffraction peak, indicating that pure KTN has no defects and is a perfect crystal. 2+ The electronic configuration is 1S22S22P63S23P63d9, with an unpaired electron in the outer layer. The orange curve is the yellow-green Cu-KTN single crystal detected by EPR, with obvious unpaired electron signals. The peak at position 3500G is Cu 2+ Ion signal. It can be judged that the yellow-green Cu-KTN single crystal contains a certain amount of Cu 2+ In contrast, the purple curve of the reddish-brown crystal after 405nm light excitation shows that the characteristic peak becomes significantly smaller, indicating that the number of unpaired electrons decreases. This indicates that the valence state of Cu after excitation is Cu + (1S22S22P63S23P63d10) or Cu 0 (1S22S22P63S23P63d104S1). The characteristic peak of the green curve after green light irradiation is enhanced, indicating that the number of unpaired electrons increases and the divalent Cu 2+ Increased content.

[0073] The XAFS of the Cu-KTN crystal prepared in Example 1 is as follows: Figure 7 As shown. In order to further reveal the chemical state of Cu, X-ray absorption fine structure (XAFS) analysis was performed. Using Cu foil (Cu foil), CuO and Cu2O as reference materials, the Cu K-edge X-ray absorption near edge structure (XANES) spectrum of Cu-KTN after 405nm light excitation was studied. Figure 7As shown in a, the Cu k-edge of Cu-KTN is very close to the Cu k-edge of Cu foil, which indicates that the valence state of Cu in Cu-KTN after UV excitation tends to be Cu 0 .from Figure 7 In b, it can be seen that the Fourier transform (FT) k3-weighted χ(k) function of the extended x-ray absorption fine structure (EXAFS) spectrum of Cu-KTN is The dominant peak of Cu-Cu coordination is shown at 405 nm, which confirms that the Cu in Cu-KTN after 405 nm photoexcitation 0 As is known to all, fitting the EXAFS data can obtain information such as the coordination and bond length of the corresponding elements, and wavelet transform analysis can distinguish the coordination elements of the Cu bond length in R space. Figure 7 c shows a typical wavelet transform of CuK edge, and 7d is the a-space result obtained by EXAFS fitting of Cu K edge. The specific fitting data is that the coordination number of Cu atom is about 12 and the average bond length is The Cu-KTN crystal is yellow-green Cu 2+ Turns to reddish brown Cu 0 , 405nm light irradiation causes KTN to undergo a valence change reaction to generate zero-valent Cu.

[0074] The deflection performance of the KTN crystal prepared in Comparative Example 1 is as follows Figure 8 As shown, the deflection performance of the Cu-KTN crystal prepared in Example 1 is as follows Figure 8 As shown, the laser uses a 633nm red collimated beam, and the polarizer has an up-and-down polarization direction, which is parallel to the electric field direction. Figure 8 As shown in a, the deflection angles of KTN and Cu-KTN crystals under applied voltage. It can be seen that when there is no laser irradiation, the deflection angle increases as the voltage increases. And the deflection angle of Cu-KTN (18.6mrad, 1400v) crystal is greater than that of pure KTN (14.82mrad, 1400v) crystal. According to the lattice distortion caused by Cu doping calculated from the first principles above, the polarization intensity increases, making the dielectric constant of Cu-KTN large, so the deflection angle under applied voltage is greater than that of KTN. Figure 8 As shown in b, it is the deflection angle of KTN and Cu-KTN crystals under the same voltage but different light powers. As the 405nm light power increases, the deflection angle of pure KTN crystal increases. This shows that the greater the photon energy, the greater the kinetic energy of the electron absorbing energy, and the greater the possibility of electrons escaping from trapped quantum wells. As the light current density increases, the free charge density increases. The deflection angle is proportional to the charge density, so the deflection angle increases. The increase in the light irradiation deflection angle of Cu-KTN (13.3mrad, 40mW) crystal is much greater than that of pure KTN (9.6mrad, 40mW). Figure 5The absorption spectrum of a shows that the bandgap width of Cu-KTN is reduced. This indicates that the energy required for the photoinduced transition electrons of Cu-KTN is small, and more electrons are excited at the same photon energy. When 405nm light irradiates green Cu-KTN, the electrons in the O2p orbit are excited, and some of the electrons are captured by the electron defects in the crystal and temporarily stored. At the same time, the electrons captured by the defects are transferred to Cu 2+ Upper, Cu 2+ Gain electrons and be reduced to Cu 0 At this time, Cu-KTN turns reddish brown. Figure 4 As shown in Figure d, Cu doping increases the photocurrent of KTN. This indicates that the charge density of Cu-KTN is greater than that of KTN, which increases the number of electrons injected under voltage and the injection depth. Doping with Cu ions makes KTN more conducive to the flipping of PNR under the action of an electric field. The experimentally measured deflection angle is in good agreement with the results of theoretical analysis, proving the feasibility of increasing the deflection angle of photochromic Cu-doped KTN crystals.

[0075] Example 10

[0076] (1) Configuration component is KTa 0.6 Nb 0.4 The amount of O3 raw materials, CuO, Fe2O3, K2CO3, Ta2O5, Nb2O5 molar ratio is 0.01:0.005:0.49:0.3:0.2, after being mixed and stirred evenly, it is placed in a muffle furnace at 900℃ for pre-sintering for 12h. The platinum crucible containing the pre-sintered product is placed in the center of the temperature field of the crystal growth furnace. The temperature amplitude is accurately controlled at 0.2℃ by the pulling method, the pulling speed is controlled at about 0.3mm / h, and the growth temperature is 1300℃.

[0077] (2) After the crystal growth is completed in one week, the temperature is lowered to room temperature to obtain a large Fe-Cu-KTN single crystal. The crystal is oriented, cut, and polished into Fe-Cu-KTN crystals of a certain size for later use.

[0078] Embodiment 11

[0079] (1) Configuration component is KTa 0.6 Nb 0.4 The amount of O3 raw materials, Fe2O3: K2CO3, Ta2O5, Nb2O5 molar ratio is 0.01:0.99:0.6:0.4, after being mixed and stirred evenly, it is placed in a muffle furnace at 900℃ for pre-sintering for 12h. The platinum crucible containing the pre-sintered product is placed in the center of the temperature field of the crystal growth furnace. The temperature amplitude is accurately controlled at 0.2℃ by the pulling method, the pulling speed is controlled at about 0.3mm / h, and the growth temperature is 1300℃.

[0080] (2) After the crystal growth is completed in one week, the temperature is lowered to room temperature to obtain a large Fe-KTN single crystal. The crystal is oriented, cut, and polished into Fe-KTN crystals of a certain size for later use.

[0081] The Fe-Cu-KTN crystal obtained in Example 10 was also observed to change color after irradiation with 405nm ultraviolet light, and after irradiation with green light or red light, and the process can be reversibly controlled. The Fe-KTN crystal obtained in Example 11 is light yellow and has no photochromic phenomenon. This shows that only Cu doped KTN or Cu doped with other elements KTN produces photochromism. In addition, it can be seen from the above that the reason why KTN single crystal is photochromic is that KTN is doped with copper, so when copper is combined with other elements, photochromism can also be produced. The fact that Cu can be doped with other elements in KTN also makes it possible for KTN crystals to change in multiple colors.

[0082] In addition, the Cu-doped KTN crystal of the present invention can be applied to a crystal modulator, and can be used to modulate the photoelectric field and light intensity in an optical path.

[0083] Although the present invention has been described in detail by referring to the accompanying drawings and in combination with the preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and these modifications or substitutions shall be within the scope of the present invention. Any person of ordinary skill in the art may easily think of changes or substitutions within the technical scope disclosed by the present invention, and these shall be within the scope of protection of the present invention. Therefore, the scope of protection of the present invention shall be subject to the scope of protection of the claims.

Claims

1. A photochromic copper-doped KTN single crystal, Features: The molecular formula of the KTN single crystal is M:KTa 1- x Nb x O 3 ; M is Cu or a combination of Cu and Fe; 0<x<1, the doping ion concentration ratio of Cu is>0; When M is Cu, when the single crystal is irradiated with ultraviolet light of 405nm or less, the color changes from yellow-green to red-brown, and after the irradiation stops, the color gradually returns to yellow-green; when irradiated with green or red light, the color changes to light green, and after the irradiation stops, the color gradually returns to yellow-green; The method for preparing the photochromic copper-doped KTN single crystal comprises the following steps: (1) KTa doped with Cu or Cu and Fe as required 1-x Nb x O 3 The ratio of configuration Ta 2 O 5 , Nb 2 O 5 , K 2 CO 3 , CuO or Cu 2 At least one of O and Cu, optionally Fe 2 O 3 The raw materials are mixed and stirred uniformly, and then placed in a furnace for pre-sintering; the crucible containing the pre-sintered product is placed in the center of the temperature field of the crystal growth furnace; the temperature amplitude, pulling speed and growth temperature are controlled by the pulling method; (2) After 7-10 days of crystal growth, the temperature is cooled to room temperature to obtain a Cu-KTN or Cu-Fe-KTN single crystal; The pre-sintering temperature of step (1) is 800-1000 0 C; The pulling speed of step (1) is 0.01 mm / h-2 mm / h, and the growth temperature of step (1) is 1000-1500 o C.

2. The photochromic copper-doped KTN single crystal according to claim 1, Features: The ratios of the elements are Cu:K:Ta:Nb:O=0.01:0.99:0.595:0.405:

3.

3. The photochromic copper-doped KTN single crystal according to claim 1, It is characterized in that Ta described in step (1) 2 O 5 , Nb 2 O 5 The molar ratio is 1-x:x.

4. The photochromic copper-doped KTN single crystal according to claim 1, It is characterized in that The temperature range of step (1) is 0.2-1 o C.

5. The photochromic copper-doped KTN single crystal according to claim 1, It is characterized in that The CuO or Cu or Cu in step (1) 2 O in M:KTa per mol 1-x Nb x O 3 The molar amount of Cu is added in a ratio of 0.001%~20%.

6. The photochromic copper-doped KTN single crystal according to claim 1, It is characterized in that The following steps are involved: (1) The configuration composition is Cu:KTa 0.6 Nb 0.4 O 3 The amount of raw materials, CuO, K 2 CO 3 、 2 O 5 , Nb 2 O 5 The molar ratio is 0.01:0.495:0.3:0.

2. After mixing and stirring evenly, place it at 900 0 C muffle furnace for 12 hours; the platinum crucible containing the pre-sintered product is placed in the center of the temperature field of the crystal growth furnace, and the temperature amplitude is accurately controlled within 0.2 o C, the pulling speed is controlled at 0.3mm / h, and the growth temperature is 1300 0 C; (2) After the crystal growth is completed in one week, the temperature is cooled to room temperature to obtain a large Cu-KTN single crystal; (3) Orient, cut, and polish the crystal into Cu-KTN crystals of a certain size for later use.

7. Use of the photochromic copper-doped KTN single crystal according to any one of claims 1 to 6, Features: The single crystal is applied to the field of photochromism or the field of increasing the deflection angle of a light beam.