Borosilicate glass and preparation method thereof

By adding glass powder and hot pressing treatment in the preparation of borosilicate glass, a protective layer is formed to reduce the volatilization of B2O3, which solves the problem of high B2O3 volatilization rate during the melting process of borosilicate glass, improves product quality and furnace life, and simplifies process.

CN117303733BActive Publication Date: 2024-10-29QINGYUAN CSG NEW ENERGY SAVING MATERIALS CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311252249.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-26
Publication Date
2024-10-29
Estimated Expiration
2043-09-26

AI Technical Summary

Technical Problem

B2O3 is easy to volatilize during the melting process of borosilicate glass, resulting in large loss of raw materials, reduced product quality and shortened furnace service life. The traditional method of reducing boron volatilization is complex and ineffective.

Method used

Provides a method for preparing borosilicate glass, by adding glass powder with a particle size of ≤75 μm to the first batch of borosilicate glass composition requirements to form a protective layer to reduce B2O3 volatilization, and improve the molding material through hot pressing treatment. density and melting efficiency.

Benefits of technology

It effectively reduces the volatilization rate of B2O3, improves the quality of glass products, extends the service life of the furnace, and simplifies the process. It is suitable for borosilicate glass with different formulas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to a borosilicate glass and a preparation method thereof. The preparation method of borosilicate glass comprises the following steps: providing a first batch material containing a SiO2 source and a B2O3 source according to the component requirements of borosilicate glass; adding glass powder to the first batch material to prepare a second batch material, wherein the mass fraction of the glass powder in the second batch material is 4% to 40%, and the particle size of the glass powder is ≤75 μm; and melting, clarifying and annealing the second batch material to prepare borosilicate glass. In the preparation method, when the second batch material is melted, the glass powder has a low softening temperature and a small particle size, and is easy to quickly soften into a liquid phase with a certain adhesiveness, and forms a protective layer that wraps the first batch material, so that the volatile components in the first batch material can be adsorbed and melted in the protective layer, thereby achieving the purpose of reducing the volatility of B2O3 from the source.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of glass, and in particular to borosilicate glass and a preparation method thereof. Background Art

[0002] Compared with ordinary glass, SiO in borosilicate glass 2 With B 2 O 3 It has a higher content, a lower thermal expansion coefficient, higher thermal shock resistance and higher surface hardness, and performs better in thermal stability, chemical stability, optical properties, mechanical properties and processing properties. It can be used in architectural fireproof glass, instrument glass, pharmaceutical glass, display panel glass, solar vacuum collector tube glass and electronic equipment substrate glass.

[0003] B 2 O 3 It is a key component in borosilicate glass, which can improve a series of properties of glass and has good fluxing properties. 2 O 3 It is easy to volatilize, causing the molten glass to change and deteriorate, making the actual composition of borosilicate glass very different from the target composition. 2 O 3 The volatilization of carbon dioxide will not only consume a large amount of raw materials and reduce product quality, but also have great corrosiveness to the furnace, seriously shortening the service life of the furnace. Summary of the invention

[0004] Based on this, it is necessary to provide a borosilicate glass and a preparation method thereof to overcome the problem of B in the glass melting process. 2 O 3 It is easy to volatilize, resulting in the loss of a large amount of raw materials, reduced product quality and shortened the service life of the furnace.

[0005] The above object of the present invention is achieved through the following technical solutions:

[0006] In a first aspect of the present invention, a method for preparing borosilicate glass is provided, comprising the following steps:

[0007] According to the composition requirements of borosilicate glass, we provide 2 Source and B 2 O 3 A first batch material of the source;

[0008] Adding glass powder to the first batch material to prepare a second batch material, wherein the mass fraction of the glass powder in the second batch material is 4% to 40%, and the particle size of the glass powder is ≤75 μm;

[0009] The second batch material is melted, clarified and annealed to prepare the borosilicate glass.

[0010] In one embodiment, before the second batch material is melted, clarified and annealed, the following steps are also included:

[0011] The second batch material is subjected to hot pressing treatment to obtain a molding material.

[0012] In one embodiment, the temperature of the hot pressing treatment is 400° C. to 1100° C.; and / or,

[0013] The pressure of the hot pressing treatment is 0.05MPa~1.1MPa; and / or,

[0014] The time of the hot pressing treatment is 5min to 40min.

[0015] In one embodiment, the mean square error of the titrated total alkalinity of the second batch material is ≤0.52.

[0016] In one embodiment, the first batch material also contains Al 2 O 3 Source, Na 2 O source, K 2 O source, CaO source, MgO source and La 2 O 3 One or more sources.

[0017] In one embodiment, before the second batch material is melted, clarified and annealed, the following steps are also included:

[0018] A clarifier is added to the second batch material.

[0019] In one embodiment, the glass powder comprises SiO 2 、Al 2 O 3 , B 2 O 3 、Na 2 O.K 2 O, CaO, MgO and La 2 O 3 One or more of .

[0020] In one embodiment, the melting temperature is 1600° C. to 1700° C.; and / or,

[0021] The melting time is 30 min to 120 min.

[0022] In one embodiment, the clarification temperature is 1500° C. to 1600° C.; and / or,

[0023] The clarification time is 120 min to 240 min.

[0024] In one embodiment, the annealing temperature is 600° C. to 700° C.; and / or,

[0025] The annealing time is 10 min to 60 min.

[0026] A second aspect of the present invention provides a borosilicate glass, characterized in that it is prepared using the above-mentioned method for preparing borosilicate glass.

[0027] In one embodiment, the borosilicate glass comprises the following components by mass fraction:

[0028] SiO 2 70%~80%;

[0029] Al 2 O 3 2%~10%;

[0030] B 2 O 3 5%~15%

[0031] Na 2 O2%~10%;

[0032] CaO2%~8%;

[0033] K 2 O0.1%~2%.

[0034] The present invention has the following beneficial effects:

[0035] The present invention first provides a SiO 2 Source and B 2 O 3 The first batch material is prepared as a source, and then glass powder with a particle size of ≤75μm is added to the first batch material to prepare a second batch material; when the second batch material is melted, the glass powder has a low softening temperature and a small particle size, and is easy to quickly soften into a liquid phase with a certain adhesion, and forms a protective layer that wraps the first batch material, so that the volatile components in the first batch material can be adsorbed and dissolved in the protective layer, thereby reducing B from the source. 2 O 3 The purpose of volatility is to control the mass fraction of glass powder to 4%~40%. It can be used as a filler to fill the gap between raw materials, reduce material stratification, and improve the uniformity of the second batch. Therefore, it is not necessary to add additional water to improve the uniformity, thereby avoiding the increase in water content and the impact on B 2 O 3 Adverse effects on volatility. DETAILED DESCRIPTION

[0036] In order to make the above-mentioned purpose, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.

[0037] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0038] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0039] The traditional energy-saving methods of the glass industry focus on the insulation of glass kilns, improving the combustion efficiency of fuels, and recycling waste heat, but ignore the energy saving from the perspective of improving raw materials. Optimizing the composition, content, and particle size of glass raw materials can improve the quality of glass products, reduce the melting temperature, and greatly improve thermal efficiency. Among them, the granulation of glass batch materials is an effective means to improve glass melting efficiency and reduce energy consumption.

[0040] When producing borosilicate glass, the B in the glass batch 2 O 3 It is easy to volatilize during the melting process, causing a large loss of raw materials, reducing the quality of glass products, corroding the glass kiln and shortening its service life. Traditional technology focuses on how to reduce B 2 O 3 A series of research works have been carried out on the issue of volatilization rate.

[0041] Some literature suggests that the melting temperature has an effect on B 2 O 3 The influence of volatilization is mainly manifested in the low temperature stage (before 1000℃). When glass liquid is formed, B 2 O 3The volatility is very small; when the melting temperature is 1000℃, with the increase of holding time, B 2 O 3 The volatility also gradually increased, and after the holding time reached 4h, B 2 O 3 The volatility tends to be flat, so shortening the insulation time can reduce B 2 O 3 When boric acid is used as raw material, dry pressing of the batch can effectively reduce B 2 O 3 Volatility, pressure will also affect B 2 O 3 The volatility rate is most suitable when the pressure is 30MPa.

[0042] It is suggested in the literature that the thermogravimetric curve of glass batch material shows that the addition of rare earth oxide La 2 O 3 It can effectively reduce the volatilization of boron; the mixture of boric acid and lanthanum oxide appears a new phase LaBO after heat treatment at 650℃ for 4h 3 , and some boric acid and lanthanum oxide remain, and the temperature is raised to 800℃ to continue the reaction to generate La(BO 2 ) 3 The saturated vapor pressure of lanthanum borate is small, thus reducing the volatility of boron.

[0043] There are some literatures on the impact of B 2 O 3 Multiple process factors of volatility suggest that during the glass melting process, the amount of boron volatilization mainly depends on the moisture content of the batch and the melting temperature, and the effect of temperature on volatilization is mainly manifested in the low temperature section (before 1000°C); granulation or briquetting pretreatment of the batch cannot reduce boron volatilization; pretreatment of the raw materials to form borates with a higher melting point is an effective way to reduce boron volatilization.

[0044] At the same time, some reports have shown that the effect of reducing boron volatilization can be achieved by controlling parameters such as the heating rate during melting, the feeding temperature, the melting temperature, the melting time, and the clarification time. 2 O 3 The volatilization rate can be controlled in the range of 1%~9%; there are some reports on optimizing the raw materials, components, content and hydroxyl absorption coefficient (β~OH value) of glass.

[0045] However, the above technology has the following limitations: 1) Pretreatment of the batch material for tableting inhibits B 2 O 3 The volatilization effect of boron is limited and the problem of boron volatilization cannot be fundamentally solved; 2) Adding rare earth oxide La 2 O 3It is not applicable to all borosilicate glasses, and requires targeted regulation based on the purpose and performance requirements of borosilicate glass, so its scope of application is relatively limited; 3) The effect of reducing boron volatilization through optimization in terms of component adjustment, melting process and feeding conditions is also not ideal, and the production process is relatively complex and difficult to promote.

[0046] Based on this, the first aspect of the present invention provides a method for preparing borosilicate glass to solve the problem of B 2 O 3 It is easy to volatilize, resulting in the loss of a large amount of raw materials, reduced product quality and shortened furnace service life. At the same time, it overcomes the problems of traditional methods of reducing boron volatilization, such as complex process, poor effect of inhibiting volatilization and limited application scope.

[0047] In some embodiments, the method for preparing borosilicate glass comprises the following steps:

[0048] According to the composition requirements of borosilicate glass, we provide 2 Source and B 2 O 3 A first batch material of the source;

[0049] Adding glass powder to the first batch material to prepare a second batch material, wherein the mass fraction of the glass powder in the second batch material is 4% to 40%, and the particle size of the glass powder is ≤75 μm;

[0050] The second batch material is melted, clarified and annealed to prepare the borosilicate glass.

[0051] The present invention first provides a SiO 2 Source and B 2 O 3 The first batch material is prepared as a source, and then glass powder with a particle size of ≤75μm is added to the first batch material to prepare a second batch material; when the second batch material is melted, the glass powder has a low softening temperature and a small particle size, and is easy to quickly soften into a liquid phase with a certain adhesion, and forms a protective layer that wraps the first batch material, so that the volatile components in the first batch material can be adsorbed and dissolved in the protective layer, thereby reducing B from the source. 2 O 3 The purpose of volatility is to control the mass fraction of glass powder to 4%~40%. It can be used as a filler to fill the gap between raw materials, reduce material stratification, and improve the uniformity of the second batch. Therefore, it is not necessary to add additional water to improve the uniformity, thereby avoiding the increase in water content and the impact on B 2 O 3 In addition, the method is applicable to borosilicate glass with different formulations, has a simple process, is easy to implement, and can be widely promoted and applied.

[0052] Exemplarily, the mass fraction of the glass powder in the batch can be 4%, 8%, 12%, 16%, 20%, 24%, 28%, 32%, 36% or 40%, etc., and the particle size of the glass powder can be 1μm, 5μm, 10μm, 15μm, 20μm, 25μm, 30μm, 35μm, 40μm, 45μm, 50μm, 55μm, 60μm, 65μm, 70μm or 75μm, etc.

[0053] Optionally, the mass fraction of the glass powder in the second batch material is 5% to 30%.

[0054] Further optionally, the mass fraction of the glass powder in the second batch material is 10% to 20%.

[0055] In some embodiments, before the second batch material is melted, clarified and annealed, the following steps are also included:

[0056] The second batch material is subjected to hot pressing treatment to obtain a molding material.

[0057] Hot pressing before melting, clarifying and annealing can make the glass powder and the raw materials in the first batch material tightly combined, so that the glass powder can wrap the first batch material, thereby further reducing B 2 O 3 After hot pressing, the bulk density of the molding material increases, the thermal conductivity increases, and the melting temperature decreases, thereby improving the melting efficiency and reducing the melting energy consumption; at the same time, hot pressing can also reduce the flying material phenomenon in the kiln, reduce the large amount of raw material waste, and reduce the erosion of the kiln by the flying material, thereby extending the service life of the kiln.

[0058] Optionally, the hot pressing treatment includes the step of placing the second batch material in a mold.

[0059] Further optionally, the mold includes a graphite mold and / or a ceramic mold.

[0060] Optionally, the diameter of the molding material is 20 mm to 40 mm, and the thickness is 10 mm to 30 mm. Exemplarily, the diameter of the molding material can be 20 mm, 22 mm, 24 mm, 26 mm, 28 mm, 30 mm, 32 mm, 34 mm, 36 mm, 38 mm or 40 mm, and the thickness can be 10 mm, 12 mm, 14 mm, 16 mm, 18 mm, 20 mm, 22 mm, 24 mm, 26 mm, 28 mm or 30 mm, etc.

[0061] Optionally, the temperature of the hot pressing treatment is 400° C. to 1100° C. For example, the temperature of the hot pressing treatment may be 400° C., 450° C., 500° C., 550° C., 600° C., 650° C., 700° C., 750° C., 800° C., 850° C., 900° C., 950° C., 1000° C., 1050° C. or 1100° C., etc.

[0062] Further optionally, the temperature of the hot pressing treatment is 600°C to 900°C.

[0063] Optionally, the pressure of the hot pressing treatment is 0.05MPa to 1.1MPa. Exemplarily, the pressure of the hot pressing treatment is 0.05MPa, 0.1MPa, 0.15MPa, 0.2MPa, 0.25MPa, 0.3MPa, 0.35MPa, 0.4MPa, 0.45MPa, 0.5MPa, 0.55MPa, 0.6MPa, 0.65MPa, 0.7MPa, 0.75MPa, 0.8MPa, 0.85MPa, 0.9MPa, 0.95MPa, 1MPa, 1.05MPa or 1.1MPa, etc.

[0064] Further optionally, the pressure of the hot pressing treatment is 0.1 MPa~0.9 MPa.

[0065] Optionally, the heat pressing treatment lasts for 5 min to 40 min. Exemplarily, the heat pressing treatment lasts for 5 min, 10 min, 15 min, 20 min, 25 min, 30 min, 35 min or 40 min.

[0066] Further optionally, the heat pressing treatment time is 10 min to 30 min.

[0067] Controlling the temperature, pressure and time of hot pressing can not only achieve the purpose of glass powder tightly wrapping other components, but also prevent factors such as too high temperature, too low pressure and too long time from damaging B 2 O 3 Negative impact on volatility.

[0068] In some embodiments, the mean square deviation of the titrated total alkalinity of the second batch material is ≤ 0.52. For example, the mean square deviation of the titrated total alkalinity of the second batch material can be 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5 or 0.52, etc.

[0069] The uniformity of the powder mixing of the second batch will affect the melting speed and uniformity of the glass. The determination methods include titration, conductivity, light reflection density and X-ray fluorescence spectrometry. Among them, the titration method is to take n samples (n ≥ 3) at different points of the second batch, dissolve them in hot water, filter them, add phenolphthalein indicator, titrate with standard hydrochloric acid solution, and convert the titrated total alkalinity into Na 2 CO 3 In the present invention, after adding glass powder to the first batch material, the mean square deviation of the titrated total alkalinity of the second batch material can be controlled within 0.52, and the uniformity of the second batch material is good, which is conducive to accelerating the melting speed of borosilicate glass and improving its uniformity.

[0070] In some embodiments, the first batch material further comprises Al 2 O 3 Source, Na 2 O source, K 2 O source, CaO source, MgO source and La 2 O 3 One or more sources.

[0071] It can be understood that the borosilicate glass can be one or more of low-alkali borosilicate glass, alkaline earth borosilicate glass, transition metal-doped borosilicate glass and rare earth-doped borosilicate glass. 2 and B 2 O 3 , the intermediate is Al 2 O 3 The exosome is selected from one or more of alkali metal oxides, alkaline earth metal oxides, transition metal oxides and rare earth metal oxides, including but not limited to: Na 2 O.K 2 O, CaO, MgO and La 2 O 3 Therefore, the raw materials of the first batch can be adjusted according to the composition requirements of the borosilicate glass.

[0072] Optionally, the SiO 2 The source includes quartz sand and / or silicate; wherein the silicate includes one or more of sodium silicate, potassium silicate, aluminum silicate and calcium silicate.

[0073] Optionally, the SiO 2 In the source, the mass fraction of particles with a diameter of 75μm~550μm is ≥92%, and the mass fraction of particles with a diameter of ≤75μm is ≤8%.

[0074] Optionally, the B 2 O 3The source includes borax and / or boric acid; wherein borax includes sodium borate decahydrate (Na 2 B 4 O 7 10H 2 O), sodium borate pentahydrate (Na 2 B 4 O 7 ·5H 2 O) and anhydrous sodium borate (Na 2 B 4 O 7 )

[0075] Optionally, the B 2 O 3 In the source, the mass fraction of particles with a diameter of 550μm~3350μm is ≥82%, the mass fraction of particles with a diameter ≤550μm is ≤10%, and the mass fraction of particles with a diameter ≤1000μm is ≤8%.

[0076] Optionally, the Al 2 O 3 Sources include aluminum oxide and / or aluminum hydroxide.

[0077] Optionally, the Al 2 O 3 In the source, the mass fraction of particles with a diameter of 25μm~150μm is ≥79%, the mass fraction of particles with a diameter ≤25μm is ≤20%, and the mass fraction of particles with a diameter ≤150μm is ≤1%.

[0078] Optionally, the Na 2 The O source includes one or more of sodium silicate, sodium carbonate and sodium bicarbonate.

[0079] Optionally, the Na 2 In the O source, the mass fraction of particles with a diameter of 550μm~3350μm is ≥83%, the mass fraction of particles with a diameter ≤550μm is ≤14%, and the mass fraction of particles with a diameter ≤1000μm is ≤3%.

[0080] Optionally, the CaO source includes one or more of dolomite, quicklime and limestone.

[0081] Optionally, in the CaO source, the mass fraction of particles with a particle size of 150 μm to 830 μm is ≥92%, and the mass fraction of particles with a particle size of ≤150 μm is ≤8%.

[0082] Optionally, the K 2 The O source includes one or more of potassium carbonate and potassium bicarbonate.

[0083] Optionally, the K 2In the O source, the mass fraction of particles with a diameter of 150μm~830μm is ≥58%, and the mass fraction of particles with a diameter of 830μm~1700μm is ≤30%.

[0084] In some embodiments, before the second batch material is melted, clarified and annealed, the following steps are further included:

[0085] A clarifier is added to the second batch material.

[0086] It can be understood that the fining agent is a component used to promote the elimination of bubbles in the molten glass during the fining process.

[0087] Optionally, the clarifier includes one or more of tin oxide, antimony oxide, cerium oxide, sodium sulfate, barium sulfate, calcium sulfate, sodium chloride, ammonium chloride, calcium fluoride and sodium fluorosilicate.

[0088] Further optionally, the clarifier includes one or more of tin oxide and sodium chloride.

[0089] Optionally, the mass fraction of the clarifier in the second batch material is 0.1%~1%.

[0090] Further optionally, the mass fraction of the clarifier in the second batch material is 0.4% to 0.6%.

[0091] In some embodiments, the glass powder comprises SiO 2 、Al 2 O 3 , B 2 O 3 、Na 2 O.K 2 O, CaO, MgO and La 2 O 3 One or more of .

[0092] It is understandable that the composition of the glass powder can be the same as that of the borosilicate glass, or it can be different from the composition of the borosilicate glass, as long as the components in the second batch after adding the glass powder can meet the composition requirements of the borosilicate glass. In some specific embodiments, the composition and content of the glass powder are the same as the composition and content of the borosilicate glass, so that the waste generated in the production process of the borosilicate glass can be recycled, the utilization rate of the raw materials can be improved, and the production cost of the borosilicate glass can be reduced.

[0093] In some embodiments, the glass powder includes the following components in mass fractions:

[0094] SiO 2 70%~80%;

[0095] Al2 O 3 2%~10%;

[0096] B 2 O 3 5%~15%;

[0097] Na 2 O2%~10%;

[0098] CaO2%~8%;

[0099] K 2 O0.1%~2%.

[0100] Optionally, the glass powder includes the following components in mass fractions:

[0101] SiO 2 72%~78%;

[0102] Al 2 O 3 4%~7%;

[0103] B 2 O 3 8%~12%;

[0104] Na 2 O4%~7%;

[0105] CaO3%~6%;

[0106] K 2 O0.2%~1%.

[0107] Further optionally, the glass powder includes the following components in mass fractions:

[0108] SiO 2 74%~76%;

[0109] Al 2 O 3 5%~6%;

[0110] B 2 O 3 9%~10%;

[0111] Na 2 O5%~6%;

[0112] CaO4%~5%;

[0113] K 2 O0.5%~0.8%.

[0114] Optionally, the melting temperature is 1600°C to 1700°C, for example, 1600°C, 1610°C, 1620°C, 1630°C, 1640°C, 1650°C, 1660°C, 1670°C, 1680°C, 1690°C or 1700°C.

[0115] Optionally, the melting time is 30 min to 120 min, for example, 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min or 120 min, etc.

[0116] Optionally, the clarification temperature is 1500°C to 1600°C, for example, 1500°C, 1510°C, 1520°C, 1530°C, 1540°C, 1550°C, 1560°C, 1570°C, 1580°C, 1590°C or 1600°C.

[0117] Optionally, the clarification time is 120 min to 240 min, for example, 120 min, 130 min, 140 min, 150 min, 160 min, 170 min, 180 min, 190 min, 200 min, 210 min, 220 min, 230 min or 240 min, etc.

[0118] Optionally, the annealing temperature is 600°C to 700°C, for example, 610°C, 620°C, 630°C, 640°C, 650°C, 660°C, 670°C, 680°C, 690°C or 700°C.

[0119] Optionally, the annealing time is 10 min to 60 min, for example, 10 min, 15 min, 20 min, 25 min, 30 min, 35 min, 40 min, 45 min, 50 min, 55 min or 60 min.

[0120] A second aspect of the present invention provides a borosilicate glass, which is prepared by the above-mentioned method for preparing borosilicate glass.

[0121] In some embodiments, the borosilicate glass includes the following components by mass fraction:

[0122] SiO 2 70%~80%;

[0123] Al 2 O 3 2%~10%;

[0124] B 2 O 3 5%~15%

[0125] Na 2 O2%~10%;

[0126] CaO2%~8%;

[0127] K 2 O0.1%~2%.

[0128] Optionally, the borosilicate glass includes the following components in mass fractions:

[0129] SiO 2 72%~78%;

[0130] Al 2 O 3 4%~7%;

[0131] B 2 O 3 8%~12%

[0132] Na 2 O4%~7%;

[0133] CaO3%~6%;

[0134] K 2 O0.2%~1%.

[0135] Further optionally, the borosilicate glass includes the following components in mass fractions:

[0136] SiO 2 74%~76%;

[0137] Al 2 O 3 5%~6%;

[0138] B 2 O 3 9%~10%

[0139] Na 2 O5%~6%;

[0140] CaO4%~5%;

[0141] K 2 O0.5%~0.8%.

[0142] The present invention is further described in detail below in conjunction with specific examples. In the following specific examples and comparative examples, the raw materials used, unless otherwise specified, are all commercially available products; the instruments used, unless otherwise specified, are all commercially available products; the processes used, unless otherwise specified, are all routinely selected by those skilled in the art. The raw materials used in the following specific examples and comparative examples meet the following conditions:

[0143] Quartz sand: The mass fraction of particles with a particle size of 75μm~550μm is ≥92%, and the mass fraction of particles with a particle size of ≤75μm is ≤8%;

[0144] Aluminum hydroxide: the mass fraction of particles with a particle size of 25μm~150μm is ≥79%, the mass fraction of particles with a particle size of ≤25μm is ≤20%, and the mass fraction of particles with a particle size of ≤150μm is ≤1%;

[0145] Borax: The mass fraction of particles with a particle size of 550μm~3350μm is ≥82%, the mass fraction of particles with a particle size of ≤550μm is ≤10%, and the mass fraction of particles with a particle size of ≤1000μm is ≤8%;

[0146] Soda ash (sodium carbonate): the mass fraction of particles with a particle size of 550μm~3350μm is ≥83%, the mass fraction of particles with a particle size of ≤550μm is ≤14%, and the mass fraction of particles with a particle size of ≤1000μm is ≤3%;

[0147] Limestone: The mass fraction of particles with a particle size of 150μm~830μm is ≥92%, and the mass fraction of particles with a particle size of ≤150μm is ≤8%;

[0148] Potassium carbonate: the mass fraction of particles with a particle size of 150μm~830μm is ≥58%, and the mass fraction of particles with a particle size of 830μm~1700μm is ≤30%;

[0149] The particle size of the glass powder is ≤75μm. The components of the glass powder include: SiO 2 , 75%; Al 2 O 3 , 5.4%; B 2 O 3 , 9.5%; Na 2 O, 5%; CaO, 4.4%; K 2 O, 0.7%.

[0150] The target composition of borosilicate glass is: SiO 2 , 75%; Al 2 O 3 , 5.4%; B 2 O 3 , 9.5%; Na 2 O, 5%; CaO, 4.4%; K 2 O, 0.7%.

[0151] Example 1

[0152] Quartz sand, aluminum hydroxide, borax, soda ash, limestone and potassium carbonate are prepared according to the target composition of borosilicate glass, and mixed evenly to prepare a first batch; glass powder and a clarifier are added to the first batch to prepare a second batch, the mass fraction of the glass powder in the second batch is 4%, and the mass fraction of the clarifier in the second batch is 0.5%; the second batch is melted at 1650°C for 1 hour, clarified at 1550°C for 3 hours, and annealed at 660°C for 0.5 hour to prepare borosilicate glass.

[0153] Example 2

[0154] The difference between this embodiment and embodiment 1 is that the mass fraction of the glass powder in the second batch material is 5%.

[0155] Example 3

[0156] The difference between this embodiment and embodiment 1 is that the mass fraction of the glass powder in the second batch material is 10%.

[0157] Example 4

[0158] The difference between this embodiment and embodiment 1 is that the mass fraction of the glass powder in the second batch material is 30%.

[0159] Example 5

[0160] The difference between this embodiment and embodiment 1 is that the mass fraction of the glass powder in the second batch material is 40%.

[0161] Example 6

[0162] The difference between this embodiment and embodiment 1 is that the mass fraction of the glass powder in the second batch material is 10%, and the second batch material is hot pressed before melting.

[0163] According to the target composition of borosilicate glass, quartz sand, aluminum hydroxide, borax, soda ash, limestone and potassium carbonate are prepared and mixed evenly to prepare a first batch; glass powder is added to the first batch to prepare a second batch, and the mass fraction of the glass powder in the second batch is 4%; the second batch is placed in a mold, and hot pressed at a temperature of 600°C and a pressure of 0.1MPa for 10 minutes to obtain a molding material; the molding material is melted at 1650°C for 1 hour, clarified at 1550°C for 3 hours, and annealed at 660°C for 0.5 hours to obtain borosilicate glass.

[0164] Example 7

[0165] The difference between this embodiment and embodiment 6 is that the conditions of the hot pressing treatment are hot pressing at a temperature of 600° C. and a pressure of 0.5 MPa for 30 minutes.

[0166] Example 8

[0167] The difference between this embodiment and embodiment 6 is that the conditions of the hot pressing treatment are hot pressing at a temperature of 600° C. and a pressure of 0.9 MPa for 20 minutes.

[0168] Example 9

[0169] The difference between this embodiment and embodiment 6 is that the conditions of the hot pressing treatment are hot pressing at a temperature of 750° C. and a pressure of 0.1 MPa for 30 minutes.

[0170] Example 10

[0171] The difference between this embodiment and embodiment 6 is that the conditions of the hot pressing treatment are hot pressing at a temperature of 750° C. and a pressure of 0.5 MPa for 20 minutes.

[0172] Embodiment 11

[0173] The difference between this embodiment and embodiment 6 is that the hot pressing treatment conditions are hot pressing at a temperature of 750° C. and a pressure of 0.9 MPa for 10 minutes.

[0174] Example 12

[0175] The difference between this embodiment and embodiment 6 is that the conditions of the hot pressing treatment are hot pressing at a temperature of 900° C. and a pressure of 0.1 MPa for 20 minutes.

[0176] Embodiment 13

[0177] The difference between this embodiment and embodiment 6 is that the hot pressing treatment conditions are hot pressing at a temperature of 900° C. and a pressure of 0.5 MPa for 10 minutes.

[0178] Embodiment 14

[0179] The difference between this embodiment and embodiment 6 is that the conditions of the hot pressing treatment are hot pressing at a temperature of 900° C. and a pressure of 0.9 MPa for 30 minutes.

[0180] Comparative Example 1

[0181] No glass powder was added to the second batch material of this comparative example, and the rest was consistent with Example 1.

[0182] Comparative Example 2

[0183] In the second batch material of this comparative example, no glass powder is added, and water with a mass fraction of 0.05% is added. Other conditions are consistent with those in Example 1.

[0184] Test Case

[0185] (1) Uniformity: Take 20 samples at different points of the second batch, dissolve them in hot water, filter them, add phenolphthalein indicator, titrate them with standard hydrochloric acid solution, and convert the titrated total alkalinity into Na 2 CO 3 The mean square deviation of the titrated total alkalinity of 20 samples was calculated, and the results are shown in Table 1; wherein, the smaller the mean square deviation of the titrated total alkalinity, the better the uniformity of the second batch material.

[0186] (2) B 2 O 3 Volatility rate: According to "7 Determination of Boron Trioxide" in "GB / T 1549-2008 Chemical Analysis Methods for Fiber Glass", the B in borosilicate glass is tested. 2 O 3 The actual content and calculated B 2 O 3 The volatilization amount and volatilization rate are shown in Table 1.

[0187] (3) Appearance: Observe whether there are many bubbles in the borosilicate glass. If so, the appearance of the borosilicate glass is recorded as NG (not good). If not, the appearance of the borosilicate glass is recorded as OK. The results are shown in Table 1.

[0188] As shown in Table 1, in Comparative Example 1, no glass powder and water were added to the second batch material, and the uniformity of the second batch material was the worst. 2 O 3 The volatility is also relatively high. In Comparative Example 2, 5% water was added, and the uniformity of the second batch was significantly improved, but 2 O 3 The volatility increased from 12.1% to 13.7%, indicating that adding water to the second batch is beneficial to improving the uniformity of the second batch, but it will also promote B 2 O 3 of volatilization.

[0189] In Examples 1 to 5, as the mass fraction of the glass powder in the second batch material increases, the uniformity of the second batch material gradually increases. 2 O 3The volatility generally shows a trend of gradually decreasing, and the lowest can reach 6.3%. Among them, the best mass fraction of glass powder is 10%, followed by 5% or 30%. When the mass fraction of glass powder is 4%, the uniformity of the second batch is poor, and when the mass fraction of glass powder is 40%, many small bubbles appear on the surface of the glass. This shows that without hot pressing treatment, adding glass powder to the second batch can not only significantly improve the uniformity of the second batch, but also greatly reduce B 2 O 3 However, if the content of glass powder is too high, it will affect the appearance of the product.

[0190] In Examples 6 to 14, the second batch material contains 10% by mass of glass powder, and the uniformity of the second batch material is in the range of 0.12 to 0.17; then the second batch material is placed in a mold for hot pressing to form a molding material with a diameter of 20 mm to 40 mm and a thickness of 10 mm to 30 mm. The borosilicate glass B 2 O 3 The volatility was maintained in the range of 1.6% to 8.4%; the best hot pressing condition was hot pressing at a temperature of 750°C and a pressure of 0.9 MPa for 10 min (ie, Example 11), followed by hot pressing at a temperature of 600°C and a pressure of 0.9 MPa for 20 min (ie, Example 8).

[0191] By adding glass powder and hot pressing treatment, B 2 O 3 The volatilization of volatile components such as B is significantly suppressed. Basically, only a small amount of volatilization occurs on the surface of the molten glass in the early stage of melting. This is because during the hot pressing process, the glass powder can quickly soften into a liquid with adhesion at a temperature of 600℃~800℃ and form a protective layer that wraps the first batch material, allowing B 2 O 3 The volatile components are adsorbed into the protective layer, directly blocking B from the source 2 O 3 Volatilization of light raw materials.

[0192] In addition, hot pressing the second batch material also has the following effects:

[0193] 1) Significantly reduce the energy consumption of melting process: For a glass melting furnace with a capacity of 200t, the specific heat capacity c of the second batch material is 9.66×10 2 J / (kg×K), the hot pressing temperature is 600℃, and the initial temperature is 30℃, it can be calculated that Q=cm∆T=1.1×10 11 J, where Q is the heat saved by the melting process, c is the specific heat capacity of the second batch material, m is the melted mass, and ∆T is the difference between the hot pressing temperature and the initial temperature.

[0194] 2) Significantly improve the melting rate: the density of the second batch is ρ 1 =1.2g / cm 3 , the density of the molding material is ρ 2 =2.0g / cm 3 , the packing gap between the molding materials is larger than the packing gap between the second batch materials, and the difference in packing density between the molding materials and the second batch materials is ρ 3 =0.5g / cm 3 , let the melting rate increase rate be M, then M=(ρ 2 −ρ 1 −ρ 3 ) / ρ 1 =25%; because after adding glass powder and performing hot pressing treatment, the density of the obtained molding material is significantly increased, the thermal conductivity rate is faster, and the final melting rate is significantly improved.

[0195] 3) Improve the utilization rate of raw materials: For a glass melting furnace with a production capacity of 200 tons, in the traditional method, the waste collection system will collect more than 1 t of the second batch material as waste every day, resulting in a large waste of resources; by adopting the preparation method of the present invention, the waste collection system can only collect less than 0.2 tons of waste every day, which can reduce 80% of the waste and has a high utilization rate of raw materials.

[0196] 4) Extend the service life of the kiln: When the second batch is sent into the kiln, flying materials often occur. The flying materials are easy to corrode the kiln grid under high temperature, resulting in a decrease in the service life of the grid. After hot pressing treatment, when the molding material is sent into the kiln for melting, the flying material phenomenon is effectively suppressed, especially B 2 O 3 The volatilization rate of highly corrosive components is also greatly reduced, the service life of the lattice body can be increased by 3 to 4 times, the life span is extended by 3 to 4 years, and the life of the kiln crown is increased by 2 years.

[0197] Table 1. Performance comparison of borosilicate glass

[0198]

[0199] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0200] The above-mentioned embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims, and the description can be used to interpret the content of the claims.

Claims

1. A method for preparing borosilicate glass, characterized in that: The following steps are involved: According to the composition requirements of borosilicate glass, a first batch material containing SiO2 source and B2O3 source is provided; Adding glass powder to the first batch material to prepare a second batch material, wherein the mass fraction of the glass powder in the second batch material is 4% to 40%, and the particle size of the glass powder is ≤75 μm; The second batch material is melted, clarified and annealed to prepare the borosilicate glass; Before the second batch material is melted, clarified and annealed, the following steps are also included: The second batch material is subjected to hot pressing treatment to obtain a molding material; During the hot pressing process, the glass powder can be quickly softened into a liquid state with adhesion at a temperature of 600° C. to 800° C., and form a protective layer that wraps the first batch material.

2. The method for preparing borosilicate glass according to claim 1, characterized in that: The temperature of the hot pressing treatment is 400°C to 1100°C.

3. The method for preparing borosilicate glass according to claim 2, characterized in that: The pressure of the hot pressing treatment is 0.05MPa~1.1MPa; and / or, The time of the hot pressing treatment is 5min to 40min.

4. The method for preparing borosilicate glass according to any one of claims 1 to 3, characterized in that: The mean square deviation of the titrated total alkalinity of the second batch material is ≤0.

52.

5. The method for preparing borosilicate glass according to claim 4, characterized in that: The first batch material also contains one or more of an Al2O3 source, a Na2O source, a K2O source, a CaO source, a MgO source and a La2O3 source.

6. The method for preparing borosilicate glass according to claim 5, characterized in that: Before the second batch material is melted, clarified and annealed, the following steps are also included: A clarifier is added to the second batch material.

7. The method for preparing borosilicate glass according to claim 6, characterized in that: The components of the glass powder include one or more of SiO2, Al2O3, B2O3, Na2O, K2O, CaO, MgO and La2O3.

8. The method for preparing borosilicate glass according to claim 7, characterized in that: The borosilicate glass comprises the following components by mass fraction: SiO2 70%~80%; Al2O3 2%~10%; B2O3 5%~15%; Na2O 2%~10%; CaO 2%~8%; K2O 0.1%~2%.

9. The method for preparing borosilicate glass according to any one of claims 1 to 3 and 5 to 8, characterized in that: The melting temperature is 1600°C to 1700°C; and / or, The melting time is 30 min to 120 min.

10. The method for preparing borosilicate glass according to claim 9, characterized in that: The clarification temperature is 1500°C to 1600°C; and / or, The clarification time is 120 min to 240 min.

11. The method for preparing borosilicate glass according to claim 10, characterized in that: The annealing temperature is 600° C. to 700° C.; and / or, The annealing time is 10 min to 60 min.

Citation Information

Patent Citations

  • On-line hot preparation method of glass batch

    CN101913752A

  • Preparation method for glass material stock and glass

    CN108726847A