A bionic composite material and a preparation method thereof

Through the injection molding process of cerium-cobalt doped hydroxyapatite and L-lactic acid, a bionic composite material that meets the mechanical performance requirements of cortical bone scaffolds is prepared, which solves the problem of insufficient compressive strength and tensile strength of existing materials and achieves Better mechanical properties.

CN117339006BActive Publication Date: 2024-10-29NANJING GENERAL HOSPITAL NANJING MILLITARY COMMAND P L A
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311543641.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-20
Publication Date
2024-10-29
Estimated Expiration
2043-11-20

AI Technical Summary

Technical Problem

Existing bionic composite materials are difficult to meet the high compressive strength and tensile strength requirements of cortical bone scaffolds.

Method used

A suspension slurry of cerium-cobalt doped hydroxyapatite and L-lactic acid (PLLA) polymer is used to prepare biomimetic composite materials through an injection molding process. The specific process parameters include cerium-cobalt doped hydroxyapatite and polymer polymerization. The weight ratio of materials is 5:5, the solid content of the suspension slurry is 40%, the inner diameter of the nozzle is 0.36mm, the injection rate is 150 μL/min, hydrothermal reaction and high temperature reaction conditions, etc.

Benefits of technology

The compressive strength and tensile strength of bionic composite materials are significantly improved and meet the mechanical performance requirements of cortical bone scaffolds.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117339006B_ABST
    Figure CN117339006B_ABST
Patent Text Reader

Abstract

Disclosed is a bionic composite material, which is obtained by injection molding a suspension slurry containing cerium-cobalt doped hydroxyapatite and a polymer; the polymer is selected from left-handed polylactic acid (PLLA). The bionic composite material can better meet the mechanical performance requirements of the cortical bone scaffold; in particular, the compressive strength and tensile strength are better.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of bionic materials and relates to a bionic composite material and a preparation method thereof. Background Art

[0002] Bone tissue is a complex three-dimensional dynamic tissue structure that is in a state of continuous reconstruction and remodeling during long-term life activities. Bones are mainly composed of bone minerals and collagen, with a ratio of about 2:1. Bone minerals mainly include hydroxyapatite, carbonated hydroxyapatite and amorphous calcium phosphate.

[0003] Bone tissue scaffolds can not only provide support for defective tissues, but also provide an external environment for cells and growth factors to achieve cell growth, migration, proliferation and differentiation, and ultimately achieve the purpose of repairing damage. Therefore, the macroscopic and microscopic structures of the scaffolds are important factors affecting the biological properties of the scaffolds, and they must have a three-dimensional porous structure while meeting certain mechanical properties.

[0004] A reasonable and feasible scaffold preparation method that can meet multiple requirements at the same time has always been the focus of all tissue engineering research. There are many preparation methods, which can be divided into two categories. One is the traditional preparation method, such as particle leaching, freeze drying, gas foaming, etc.; the other is the most rapidly developed and most promising rapid prototyping method in recent years, also known as additive manufacturing, including three-dimensional printing (3DP), selective laser sintering (SLS), fused deposition modeling (FDM), extrusion deposition modeling, motor-assisted injection molding, stereolithography (SLA), etc.

[0005] Chinese patent application CN101983728A discloses a shell porous hydroxyapatite-based bone repair material and a preparation method thereof. The shell porous hydroxyapatite-based bone repair material comprises a shell porous hydroxyapatite scaffold matrix and porous chitosan filled in the matrix. The preparation method comprises: mixing shell powder with diammonium hydrogen phosphate solution, heating, centrifugation to collect precipitation, washing and drying to obtain shell hydroxyapatite powder; mixing shell hydroxyapatite powder with polyvinyl alcohol and deionized water, stirring to obtain shell hydroxyapatite slurry; uniformly coating the shell hydroxyapatite slurry on the surface of polyurethane sponge, drying, sintering, and obtaining a shell hydroxyapatite porous scaffold; immersing the shell hydroxyapatite porous scaffold in a chitosan solution prepared with acetic acid for solidification, and vacuum freeze drying to obtain a shell porous hydroxyapatite-based bone repair material.

[0006] Chinese patent application CN109133907A discloses an artificial bone comprising hydroxyapatite whiskers and biphasic calcium phosphate and a preparation method thereof. The artificial bone uses hydroxyapatite whiskers, hydroxyapatite powder and β-tricalcium phosphate as raw materials, has an inducing effect on bone cell growth, and promotes the growth and healing of bone cells; by controlling the ratio of hydroxyapatite whiskers, hydroxyapatite powder and β-tricalcium phosphate, the strength of the artificial bone is improved; the preparation method of the artificial bone is 3D printing technology. On the one hand, 3D printing technology can tailor the shape of the scaffold for the patient according to the shape of the bone defect, getting rid of the defects of traditional mold manufacturing that requires molding first, size restrictions after molding, and high mold cost; on the other hand, the method can finely control the pore size, porosity and connectivity of the scaffold through 3D modeling, and the open porous structure and interconnected network are crucial for supplying cell nutrition, proliferation and differentiation, and tissue vascularization.

[0007] However, for cortical bone, the compressive strength is usually 120-180MPa, and the tensile strength is usually 50-150MPa. Many bone tissues made of bionic composite materials are difficult to meet the mechanical property requirements of cortical bone scaffolds. Summary of the invention

[0008] In view of the above problems, the present invention aims to provide a bionic composite material and a preparation method thereof which meets the mechanical property requirements of the cortical bone scaffold and is superior to the prior art, especially in terms of compressive strength and tensile strength.

[0009] To achieve the above objectives, on the one hand, the present invention adopts the following technical scheme: a bionic composite material, wherein the composite material is obtained by injection molding a suspension slurry containing cerium-cobalt doped hydroxyapatite and a polymer; the polymer is selected from left-handed polylactic acid PLLA.

[0010] According to the bionic composite material of the present invention, the weight ratio of cerium-cobalt doped hydroxyapatite to the high molecular polymer is (2-8): (8-2).

[0011] Advantageously, the weight ratio of cerium-cobalt doped hydroxyapatite to the high molecular weight polymer is (3-7):(7-3), and the preferred weight ratio is (4-6):(6-4).

[0012] In a specific embodiment, the weight ratio of cerium-cobalt doped hydroxyapatite to the high molecular polymer is 5:5.

[0013] According to the bionic composite material of the present invention, the solid content of the suspension slurry is 25-55%.

[0014] Advantageously, the suspension slurry has a solid content of 30-50%, preferably 35-45%.

[0015] In a specific embodiment, the solid content of the suspension slurry is 40%.

[0016] Advantageously, the suspension slurry contains no other solid components.

[0017] According to the bionic composite material of the present invention, the process parameters of the injection molding are: the inner diameter of the nozzle is 0.20-0.50 mm; and the injection rate is 100-200 μL / min.

[0018] Advantageously, the process parameters of the injection molding are: the inner diameter of the nozzle is 0.25-0.45 mm, preferably 0.30-0.40 mm; the injection rate is 120-180 μL / min, preferably 140-160 μL / min.

[0019] In a specific embodiment, the process parameters of the injection molding are: the inner diameter of the nozzle is 0.36 mm; the injection rate is 150 μL / min.

[0020] According to the bionic composite material of the present invention, the cerium-cobalt-doped hydroxyapatite is obtained by hydrothermal reaction and high-temperature reaction of calcium salt, cerium salt, cobalt salt and phosphate according to the Ca / P molar ratio = 1.10-1.45, Ce / Co molar ratio = 2 / 8-8 / 2 and (Ca+3 / 2Ce+Co) / P = 1.67.

[0021] Advantageously, the Ca / P molar ratio = 1.15-1.40, preferably 1.20-1.35; the Ce / Co molar ratio = 3 / 7-7 / 3, preferably 4 / 6-6 / 4.

[0022] In a specific embodiment, the Ca / P molar ratio=1.25; the Ce / Co molar ratio=1.

[0023] According to the bionic composite material of the present invention, the hydrothermal reaction is carried out under the condition of pH=9-10.

[0024] Advantageously, the hydrothermal reaction is carried out at pH = 9.2-9.8, preferably 9.3-9.7.

[0025] In a specific embodiment, the hydrothermal reaction is carried out at pH=9.5.

[0026] According to the bionic composite material of the present invention, the hydrothermal reaction conditions are: 100-250 °C hydrothermal reaction for 8-96 h.

[0027] Advantageously, the hydrothermal reaction conditions are: 120-220 °C, preferably 160-200 °C; hydrothermal reaction time 16-80 h, preferably 32-64 h.

[0028] In a specific embodiment, the hydrothermal reaction conditions are: 180 °C hydrothermal reaction for 48 h.

[0029] According to the bionic composite material of the present invention, the high temperature reaction condition is: 450-750 °C for 2-8 h.

[0030] Advantageously, the high temperature reaction conditions are: 500-700 ° C for 4-6 h, preferably 550-650 ° C for 5-7 h.

[0031] In a specific embodiment, the high temperature reaction conditions are: 600 ° C for 6 h.

[0032] In another aspect, the present invention provides a method for preparing the biomimetic composite material according to the present invention, comprising:

[0033] Cerium-cobalt doped hydroxyapatite is obtained by hydrothermal reaction and high temperature reaction of calcium salt, cerium salt, cobalt salt and phosphate according to Ca / P molar ratio = 1.10-1.45, Ce / Co molar ratio = 2 / 8-8 / 2 and (Ca+3 / 2Ce+Co) / P = 1.67;

[0034] The cerium-cobalt doped hydroxyapatite and the high molecular polymer are mixed to obtain a suspension slurry;

[0035] The suspension slurry is injection molded to obtain the bionic composite material.

[0036] Compared with the prior art, the present invention provides a bionic composite material and a preparation method thereof that better meets the mechanical property requirements of a cortical bone scaffold; and in particular, has better compressive strength and tensile strength. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 This is a SEM photo of the bionic composite material obtained in Example 1. DETAILED DESCRIPTION

[0038] It must be noted that, as used in this specification and the appended claims, the singular forms "a", "an", and "the" may include both one and plural referents (i.e., more than two, including two), unless the context clearly dictates otherwise.

[0039] Unless otherwise indicated, the numerical range in the present invention is approximately, and therefore may include values ​​outside the range. The numerical range can be expressed in the present invention as from "about" a specific value and / or to "about" another specific value. When expressing such a range, another aspect includes from the specific value and / or to another specific value. Similarly, when a value is expressed as an approximation by using the antecedent "about", it should be understood that the specific value forms another aspect. It should also be understood that the endpoint of each in the numerical range is important and independent of the other endpoint in the relationship with the other endpoint.

[0040] References in the specification and the appended claims to parts by weight of a particular element or component in a composition or article refer to the weight relationship between that element or component and any other elements or components in the composition or article expressed in parts by weight.

[0041] In the present invention, unless otherwise specifically indicated, or implied by the context or the customary manner in the technical field, the solutions mentioned in the present invention are all aqueous solutions; when the solute of the aqueous solution is a liquid, all fractions and percentages are calculated by volume, and the volume percentage of the component is based on the total volume of the composition or product containing the component; when the solute of the aqueous solution is a solid, all fractions and percentages are calculated by weight, and the weight percentage of the component is based on the total weight of the composition or product containing the component.

[0042] The terms "comprising", "including", "having" and the like mentioned in the present invention are not intended to exclude the existence of any optional components, steps or procedures, regardless of whether any optional components, steps or procedures are specifically disclosed. For the avoidance of any doubt, all methods claimed by using the term "comprising" may include one or more additional steps, equipment parts or components and / or substances unless otherwise stated. In contrast, the term "consisting of" excludes any components, steps or procedures that are not specifically described or listed. Unless otherwise stated, the term "or" refers to the members listed individually and in any combination.

[0043] Furthermore, the contents of any patent or non-patent document referenced in this invention are hereby incorporated by reference in their entirety, particularly with respect to definitions published in the art (to the extent not inconsistent with any definitions specifically provided herein) and common knowledge.

[0044] In the present invention, unless otherwise indicated, parts are by weight, temperatures are expressed in ° C or at ambient temperature, and pressures are atmospheric or near atmospheric. Room temperature means 20-30 ° C. There are many variations and combinations of reaction conditions (e.g., component concentrations, desired solvents, solvent mixtures, temperature, pressure, and other reaction ranges) and conditions that can be used to optimize the product purity and yield obtained by the method. Only reasonable routine experiments will be required to optimize such process conditions.

[0045] The following examples are merely intended to illustrate the embodiments of the present invention, rather than to limit the scope of protection of the invention.

[0046] Example 1

[0047] Calcium nitrate, cerium nitrate hexahydrate, cobalt nitrate hexahydrate and potassium dihydrogen phosphate were prepared into 1 M aqueous solutions respectively, and added into the reactor according to the molar ratio of Ca / P = 1.25, the molar ratio of Ce / Co = 1 and (Ca+3 / 2Ce+Co) / P = 1.67, and the pH value was adjusted to 9.5 and stirred for 2 h. Hydrothermal reaction was carried out at 180 °C for 48 h. Cooled to room temperature and filtered. The precipitate was washed with deionized water 3 times, and after washing, it was vacuum dried for 24 h. Placed in an electric furnace, heated to 600 °C, the heating rate was 5 °C / min, the heat preservation time was 6 h, and the temperature was cooled to room temperature with the furnace to obtain cerium cobalt doped hydroxyapatite.

[0048] 1 part of cerium-cobalt-doped hydroxyapatite and 1 part of left-handed polylactic acid (PLLA) were dispersed in chloroform and dispersed evenly by ultrasound to obtain a suspension slurry with a solid content of 40%. The suspension slurry was loaded into a micro-electric syringe and injected to obtain a bionic composite material. The process parameters of injection molding were: the inner diameter of the nozzle was 0.36 mm; the injection rate was 150 μL / min. Figure 1 The SEM photograph of the biomimetic composite material obtained in Example 1 is shown.

[0049] Comparative Example 1

[0050] Calcium nitrate, cerium nitrate hexahydrate and potassium dihydrogen phosphate were prepared into 1 M aqueous solutions respectively, and added into the reactor according to the Ca / P molar ratio = 1.25 and (Ca+5 / 2Ce) / P = 1.67, and the pH value was adjusted to 9.5, and stirred for 2 h. Hydrothermal reaction was carried out at 180 °C for 48 h. Cooled to room temperature and filtered. The precipitate was washed with deionized water for 3 times, and then vacuum dried for 24 h. Placed in an electric furnace, heated to 600 °C, the heating rate was 5 °C / min, the heat preservation time was 6 h, and cooled to room temperature with the furnace to obtain cerium-doped hydroxyapatite.

[0051] 1 part of cerium-doped hydroxyapatite and 1 part of L-polylactic acid (PLLA) were dispersed in chloroform and dispersed evenly by ultrasound to obtain a suspension slurry with a solid content of 40%. The suspension slurry was loaded into a micro-electric syringe and injected to obtain a bionic composite material. The process parameters of injection molding were: the inner diameter of the nozzle was 0.36 mm; the injection rate was 150 μL / min.

[0052] Comparative Example 2

[0053] Calcium nitrate, cobalt nitrate hexahydrate and potassium dihydrogen phosphate were prepared into 1 M aqueous solutions respectively, and added into the reactor according to the Ca / P molar ratio = 1.25 and (Ca+5 / 2Co) / P = 1.67, and the pH value was adjusted to 9.5, and stirred for 2 h. Hydrothermal reaction was carried out at 180 °C for 48 h. Cooled to room temperature and filtered. The precipitate was washed with deionized water for 3 times, and then vacuum dried for 24 h. Placed in an electric furnace, heated to 600 °C, the heating rate was 5 °C / min, the heat preservation time was 6 h, and cooled to room temperature with the furnace to obtain cobalt-doped hydroxyapatite.

[0054] 1 part of cobalt-doped hydroxyapatite and 1 part of L-polylactic acid (PLLA) were dispersed in chloroform and dispersed evenly by ultrasound to obtain a suspension slurry with a solid content of 40%. The suspension slurry was loaded into a micro-electric syringe and injected to obtain a bionic composite material. The process parameters of injection molding were: the inner diameter of the nozzle was 0.36 mm; the injection rate was 150 μL / min.

[0055] Comparative Example 3

[0056] Calcium nitrate, cerium nitrate hexahydrate, cobalt nitrate hexahydrate and potassium dihydrogen phosphate were prepared into 1 M aqueous solutions respectively, and added into the reactor according to the molar ratio of Ca / P = 1.25, the molar ratio of Ce / Co = 1 and (Ca+3 / 2Ce+Co) / P = 1.67, and the pH value was adjusted to 9.5 and stirred for 2 h. Hydrothermal reaction was carried out at 180 °C for 48 h. Cooled to room temperature and filtered. The precipitate was washed with deionized water 3 times, and after washing, it was vacuum dried for 24 h. Placed in an electric furnace, heated to 600 °C, the heating rate was 5 °C / min, the heat preservation time was 6 h, and the temperature was cooled to room temperature with the furnace to obtain cerium cobalt doped hydroxyapatite.

[0057] 1 part of cerium-cobalt-doped hydroxyapatite and 1 part of poly(lactic acid) PLLA were dispersed in chloroform and dispersed evenly by ultrasound to obtain a suspension slurry with a solid content of 20%. The suspension slurry was loaded into a micro-electric syringe and injected to obtain a bionic composite material. The process parameters of injection molding were: the inner diameter of the nozzle was 0.36 mm; the injection rate was 150 μL / min.

[0058] Performance Testing

[0059] The compressive strength and tensile strength of the biomimetic composite materials obtained in the examples and comparative examples were measured using a universal material testing machine, both in MPa. The results are shown in Table 1.

[0060] Table 1

[0061] It should be understood that the specific embodiments of the present invention are only used to illustrate the spirit and principles of the present invention, and are not used to limit the scope of the present invention. In addition, it should be understood that after reading the content of the present invention, those skilled in the art can make various changes, substitutions, deletions, corrections or adjustments to the technical solutions of the present invention, and these equivalent technical solutions also fall within the scope defined by the claims of the present invention.

Claims

1. A biomimetic composite material, wherein: The composite material is obtained by injection molding a suspension slurry containing cerium-cobalt doped hydroxyapatite and a high molecular polymer; the high molecular polymer is selected from left-handed polylactic acid PLLA; The weight ratio of cerium-cobalt doped hydroxyapatite to high molecular weight polymer is (2-8): (8-2); The cerium-cobalt doped hydroxyapatite is obtained by hydrothermal reaction and high temperature reaction of calcium salt, cerium salt, cobalt salt and phosphate according to the molar ratio of Ca / P=1.10-1.45, the molar ratio of Ce / Co=2 / 8-8 / 2 and (Ca+3 / 2Ce+Co) / P=1.67; The hydrothermal reaction was carried out at pH = 9-10; The hydrothermal reaction conditions are: 100-250 °C hydrothermal reaction for 8-96 h; The high temperature reaction conditions are: 450-750 ° C for 2-8 h; The solid content of the suspension slurry is 25-55%.

2. The biomimetic composite material according to claim 1, wherein: The solid content of the suspension slurry is 30-50%.

3. The biomimetic composite material according to claim 2, wherein: The solid content of the suspension slurry is 35-45%.

4. The biomimetic composite material according to claim 1, wherein: The process parameters of the injection molding are: the inner diameter of the nozzle is 0.20-0.50 mm; the injection rate is 100-200 μL / min.

5. A method for preparing the biomimetic composite material according to any one of claims 1 to 4, comprising: Cerium-cobalt doped hydroxyapatite is obtained by hydrothermal reaction and high temperature reaction of calcium salt, cerium salt, cobalt salt and phosphate according to Ca / P molar ratio = 1.10-1.45, Ce / Co molar ratio = 2 / 8-8 / 2 and (Ca+3 / 2Ce+Co) / P = 1.67; The cerium-cobalt doped hydroxyapatite and the high molecular polymer are mixed to obtain a suspension slurry; The suspension slurry is injection molded to obtain the bionic composite material.

Citation Information

Patent Citations

  • Shell porous hydroxyapatite basal bone repair material and preparation method thereof

    CN101983728A

  • Artificial bone containing hydroxyapatite whiskers and diphasic calcium phosphate and preparation method of artificial bone

    CN109133907A