An antiviral melamine resin material and its preparation method and application

By introducing modified titanium dioxide and quaternary ammonium salts into melamine resins, combining formaldehyde and polyethylene glycol, antiviral modified melamine resin materials are prepared, which solves the problems of poor antiviral and poor antibacterial properties and insufficient toughness of melamine resin materials. It achieves efficient antiviral and antibacterial effects and improves flexibility.

CN117343258BActive Publication Date: 2024-11-15CLEANSPACE(CHINA) LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202311296204.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-09
Publication Date
2024-11-15
Estimated Expiration
2043-10-09

AI Technical Summary

Technical Problem

Melamine resin materials lack antiviral and antibacterial ability under high environmental humidity, and have poor toughness, which is prone to cracking, affecting the quality of the board.

Method used

通过将纳米二氧化钛与γ-氨丙基三乙氧基硅烷、2,2-二羟甲基丙酸和二环己基碳二亚胺等物质反应,形成改性二氧化钛,并与三聚氰胺结合,引入季 Ammonium salt and formaldehyde were prepared to improve antiviral and antibacterial properties, and improve flexibility through polyethylene glycol.

Benefits of technology

This method not only improves the antiviral and antibacterial ability of the material, enhances its toughness and mechanical properties, effectively inhibits the replication and reproduction of viruses and bacteria, but also achieves the bactericidal effect through chemical grafting and physical mechanisms, significantly improving the quality of the plate .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117343258B_ABST
    Figure CN117343258B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of antiviral plates, and discloses an antiviral melamine resin material and a preparation method and application thereof. Nano titanium dioxide is firstly subjected to amino modification, and then reacted with 2,2-dihydroxymethyl propionic acid to obtain modified titanium dioxide, the modified titanium dioxide is reacted with triethanolamine and melamine, and then hexachlorodecane and triethanolamine are used to undergo quaternization reaction to obtain antiviral modified melamine, and the antiviral melamine resin material is reacted with formaldehyde and polyethylene glycol to obtain the antiviral melamine resin material. The nano titanium dioxide has excellent antiviral and antibacterial effects, cations on the quaternary ammonium salt are combined with anions on bacterial cell walls to kill bacteria, and polyethylene glycol is a linear diol with excellent flexibility, and a cross-linked network melamine resin material is generated, the activity of the molecular chain is high, the cross-linking density of the resin is reduced, the bendability is increased, and the flexibility of the melamine resin is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of antiviral boards, in particular to an antiviral melamine resin material and a preparation method and application thereof. Background Art

[0002] Melamine resin (MF) is a thermosetting amino resin with good hardness, thermal stability, transparency, water resistance and weather resistance. It is widely used in outdoor board coatings, wood flooring decorative layers and veneer products. However, in the case of high humidity, the board lacks antiviral and antibacterial capabilities and is prone to breed various pathogens. With the rapid development of my country's social economy and the continuous improvement of living and housing conditions, people are paying more and more attention to the indoor environment and the safety and health of indoor furniture. Therefore, there are higher and higher requirements for the antiviral and antibacterial properties of the board. At the same time, melamine resin is brittle and has poor flexibility. It is prone to cracking under stress, which can easily lead to quality problems in the board. Therefore, improving the flexibility of MF resin and improving its brittleness can improve the quality of the board.

[0003] Chinese patent CN103222477B discloses a silver ion inorganic antibacterial agent and a melamine resin and impregnated paper prepared with the same. The silver ion inorganic antibacterial agent used is composed of the following raw materials in parts by weight: 5 to 15 parts of a silver ion complex and 85 to 95 parts of phosphoric acid. It has good long-term antibacterial effect. When used in melamine resin, it has good stability, uniform dispersion, and no precipitation for a long time. The color of the impregnated paper processed with the obtained antibacterial paper does not change, and the antibacterial effect is good. However, the cost of the antibacterial agent is relatively high, and the toughness of the melamine resin is relatively poor.

[0004] Therefore, developing melamine resin materials with good toughness and antiviral properties is an inevitable requirement for technological progress. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides an antiviral melamine resin material and a preparation method and application thereof, which solves the problems of poor toughness, antiviral and antibacterial properties of melamine resin materials.

[0006] In order to achieve the above object, the present invention discloses a method for preparing an antiviral melamine resin material, comprising the following steps:

[0007] Step 1, ultrasonically disperse nano titanium dioxide (TiO2) in anhydrous ethanol, and after uniform dispersion, add γ-aminopropyltriethoxysilane, stir and mix, react, and after the reaction is completed, filter, wash with anhydrous ethanol, and dry in a drying oven at 80°C for 12 hours to obtain amino titanium dioxide;

[0008] Step 2: Ultrasonically disperse the amino titanium dioxide in tetrahydrofuran, and after uniform dispersion, add 2,2-dihydroxymethylpropionic acid and dicyclohexylcarbodiimide (DCC), stir and mix, and react in a nitrogen atmosphere. After the reaction is completed, rotary evaporate and vacuum dry at 60° C. for 6 hours to obtain modified titanium dioxide;

[0009] Step 3, deionized water, modified titanium dioxide and triethanolamine are mixed evenly, heated to 75°C, phosphoric acid is added to adjust the pH to 3, and melamine is added, stirred and mixed to react. After the reaction is completed, centrifugation is performed, deionized water is used for washing, and the mixture is dried at 60°C for 12 hours to obtain modified melamine;

[0010] Step 4: Acetone, modified melamine and hexadecane are stirred and mixed to react. After the reaction is completed, the obtained product is precipitated with n-heptane, and then washed with acetone, filtered, and dried to obtain antiviral modified melamine;

[0011] Step 5: Evenly mix the formaldehyde solution and the sodium hydroxide solution, adjust the pH value to 8.5-9.0, then add polyethylene glycol, melamine and antiviral modified melamine, stir and mix, react, and after the reaction is completed, obtain the antiviral melamine resin material.

[0012] Preferably, in the step 1, the mass ratio of anhydrous ethanol, nano-titanium dioxide and γ-aminopropyltriethoxysilane is 3200-4000:100:78-102.

[0013] Preferably, the reaction temperature in step 1 is 55-65° C., and the reaction time is 6-9 h.

[0014] Preferably, in the step 2, the mass ratio of the aminated titanium dioxide, tetrahydrofuran, 2,2-dihydroxymethylpropionic acid and dicyclohexylcarbodiimide is 100:1500-2100:105-180:5-9, the reaction temperature is 25-35° C., and the reaction time is 14-16 h.

[0015] Preferably, in step three, the mass ratio of deionized water, modified titanium dioxide, triethanolamine and melamine is 550-700:5-9:12-18:100.

[0016] Preferably, the reaction temperature in step 3 is 70-80° C., and the reaction time is 2-3 h.

[0017] Preferably, in step 4, the mass ratio of acetone, modified melamine and hexadecane chloride is 900-1200:100:68-95.

[0018] Preferably, the reaction temperature in step 4 is 65-75° C., and the reaction time is 3-4 h.

[0019] Preferably, in step 5, the mass ratio of the formaldehyde solution, polyethylene glycol, melamine and antiviral modified melamine is 95-115:18-24:100:9-12.

[0020] Preferably, the reaction temperature in step 5 is 75-85° C., and the reaction time is 2-3 h.

[0021] Preferably, the formaldehyde solution in step five is a formaldehyde aqueous solution with a mass concentration of 37%.

[0022] Preferably, the sodium hydroxide solution in step five is a sodium hydroxide aqueous solution with a mass concentration of 30%.

[0023] Preferably, the antiviral melamine resin material is prepared by the method for preparing the antiviral melamine resin material.

[0024] Preferably, the antiviral melamine resin material is used in indoor furniture panels and floors.

[0025] In the present invention, gamma-aminopropyltriethoxysilane is first used to carry out amino modification on nano titanium dioxide, and amino groups are introduced on the surface of the nano titanium dioxide to obtain amino titanium dioxide. The amino groups on the amino titanium dioxide and the carboxyl groups on 2,2-dihydroxymethyl propionic acid undergo amidation reaction under the action of dicyclohexylcarbodiimide. After the reaction is completed, modified titanium dioxide is obtained. The hydroxyl groups introduced on the modified titanium dioxide, the hydroxyl groups on the triethanolamine and the amino groups on the melamine react. After the reaction is completed, modified melamine is obtained. The triethanolamine introduced in the modified melamine undergoes quaternization reaction with hexadecane chloride to introduce quaternary ammonium salt to obtain antiviral modified melamine, which then reacts with formaldehyde, polyethylene glycol and melamine to obtain an antiviral melamine resin material.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] The nano titanium dioxide used in the present invention is low in price and cost of use. Due to its small size and fast migration speed, it has a very rapid sterilization rate. At the same time, the nano titanium dioxide can block the way for the virus to enter the host cell by adsorbing specific proteases on the surface of virus-infected cells, thereby inhibiting virus replication, and can also induce the body to produce an antiviral immune response, enhance the body's resistance to viral infection, and has excellent antiviral ability. Under light, the electrons on the valence band of the nano titanium dioxide can be excited to the conduction band, generate electron-hole pairs, migrate to the surface of the titanium dioxide, generate active oxygen, react with organic matter in the bacteria, oxidize it, and promote cell apoptosis. Through the chemical grafting method, the agglomeration of the nano titanium dioxide is effectively avoided. The cations on quaternary ammonium salts can combine with the anions on the bacterial cell wall, penetrate and diffuse into the interior of the bacteria, change the permeability of the bacterial cell wall, destroy the system of protein and cell membrane synthesis, and make the cells unable to produce the protein enzymes required for their own survival, thereby inhibiting the reproduction and survival of bacteria. The high-molecular quaternary ammonium salt groups with long-chain alkyl groups have better bactericidal properties than small-molecule quaternary ammonium salts. Long-chain alkanes can react hydrophobically with the lipid layer on the bacterial cells, causing the protein in the cells to denature, thereby leading to enzyme inactivation. They adsorb bacteria through high-density charges and penetrate into the lipid layer and protein layer of the bacterial cells to achieve a physical mechanism of bactericidal effects. At the same time, they have obvious synergistic effects on the damage and death of the lipid membrane of small microorganisms such as viruses, and have strong antibacterial and antiviral capabilities.

[0028] Nano titanium dioxide has excellent mechanical properties in the present invention, can improve the mechanical properties of matrix, and improve the toughness of matrix. Polyethylene glycol is a straight-chain dibasic alcohol with excellent flexibility, two hydroxyls on polyethylene glycol and amino groups on melamine and antiviral modified melamine are subjected to dehydration condensation, connected by flexible chains, forming a flexible preferably double-triazine ring structure, reacting with formaldehyde, generating a cross-linked networked melamine resin material, greatly improving the intramolecular deformability, the activity of the molecular chain is higher, thereby reducing the crosslinking density of the resin, and the bending property increases, improving the toughness of the resin product, and nano titanium dioxide is grafted on melamine, reacts with polyethylene glycol and formaldehyde, and is uniformly dispersed in the matrix, can form a uniform mechanical network, and improves the mechanical properties of the matrix. The long-chain alkane introduced in the quaternary ammonium salt process is introduced simultaneously and can further improve the toughness of the matrix. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a schematic diagram of the structure of the synthesized modified titanium dioxide in the present invention. DETAILED DESCRIPTION

[0030] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0031] Example 1

[0032] A method for preparing an antiviral melamine resin material comprises the following steps:

[0033] Step 1, ultrasonically disperse nano titanium dioxide in anhydrous ethanol, and after uniform dispersion, add γ-aminopropyltriethoxysilane, wherein the mass ratio of anhydrous ethanol, nano titanium dioxide and γ-aminopropyltriethoxysilane is 3200:100:78, stir and mix, react at 55°C for 9h, and after the reaction is completed, filter, wash with anhydrous ethanol, and dry in a drying oven at 80°C for 12h to obtain amino titanium dioxide;

[0034] Step 2, ultrasonically dispersing the aminated titanium dioxide into tetrahydrofuran, after uniform dispersion, adding 2,2-dihydroxymethylpropionic acid and dicyclohexylcarbodiimide, stirring and mixing, wherein the mass ratio of aminated titanium dioxide, tetrahydrofuran, 2,2-dihydroxymethylpropionic acid and dicyclohexylcarbodiimide is 100:1500:105:5, reacting at 25°C in a nitrogen atmosphere for 16 hours, after the reaction is completed, rotary evaporation, vacuum drying at 60°C for 6 hours, to obtain modified titanium dioxide;

[0035] Step 3, deionized water, modified titanium dioxide and triethanolamine are mixed evenly, heated to 75°C, phosphoric acid is added to adjust the pH to 3, and melamine is added and stirred, wherein the mass ratio of deionized water, modified titanium dioxide, triethanolamine and melamine is 550:5:12:100, and the reaction is carried out at 70°C for 3 hours. After the reaction is completed, centrifugation is performed, deionized water is used for washing, and the mixture is dried at 60°C for 12 hours to obtain modified melamine;

[0036] Step 4: Acetone, modified melamine and hexachlorodecane in a mass ratio of 900:100:68 are stirred and mixed, and reacted at 65° C. for 4 hours. After the reaction is completed, the obtained product is precipitated with n-heptane, and then washed with acetone, filtered, and dried to obtain antiviral modified melamine;

[0037] Step 5: Evenly mix a 37% formaldehyde aqueous solution and a 30% sodium hydroxide aqueous solution, adjust the pH value to 8.5, add polyethylene glycol, melamine and antiviral modified melamine, and stir to mix, wherein the mass ratio of the formaldehyde aqueous solution, polyethylene glycol, melamine and antiviral modified melamine is 95:18:100:9, react at 75° C., the reaction time is 3 hours, and after the reaction is completed, an antiviral melamine resin material is obtained.

[0038] Example 2

[0039] A method for preparing an antiviral melamine resin material comprises the following steps:

[0040] Step 1, ultrasonically disperse nano titanium dioxide in anhydrous ethanol, and after uniform dispersion, add γ-aminopropyltriethoxysilane, wherein the mass ratio of anhydrous ethanol, nano titanium dioxide and γ-aminopropyltriethoxysilane is 3500:100:85, stir and mix, react at 60°C for 7h, and after the reaction is completed, filter, wash with anhydrous ethanol, and dry in a drying oven at 80°C for 12h to obtain amino titanium dioxide;

[0041] Step 2, ultrasonically dispersing the aminated titanium dioxide into tetrahydrofuran, after uniform dispersion, adding 2,2-dihydroxymethylpropionic acid and dicyclohexylcarbodiimide, stirring and mixing, wherein the mass ratio of aminated titanium dioxide, tetrahydrofuran, 2,2-dihydroxymethylpropionic acid and dicyclohexylcarbodiimide is 100:1800:140:6.5, reacting at 30°C in a nitrogen atmosphere for 15h, after the reaction is completed, rotary evaporation, vacuum drying at 60°C for 6h, to obtain modified titanium dioxide;

[0042] Step 3, deionized water, modified titanium dioxide and triethanolamine are mixed evenly, heated to 75°C, phosphoric acid is added to adjust the pH to 3, and melamine is added and stirred, wherein the mass ratio of deionized water, modified titanium dioxide, triethanolamine and melamine is 600:6.5:14:100, and the reaction is carried out at 75°C for 2.5 hours. After the reaction is completed, centrifugation is performed, deionized water is used for washing, and the mixture is dried at 60°C for 12 hours to obtain modified melamine;

[0043] Step 4: Acetone, modified melamine and hexadecane chloride in a mass ratio of 1000:100:75 are stirred and mixed, and reacted at 60° C. for 3.5 hours. After the reaction is completed, the obtained product is precipitated with n-heptane, and then washed with acetone, filtered, and dried to obtain antiviral modified melamine;

[0044] Step 5: Evenly mix a 37% formaldehyde aqueous solution and a 30% sodium hydroxide aqueous solution, adjust the pH value to 8.8, add polyethylene glycol, melamine and antiviral modified melamine, and stir to mix, wherein the mass ratio of the formaldehyde aqueous solution, polyethylene glycol, melamine and antiviral modified melamine is 102:20:100:10, react at 80°C, the reaction time is 2.5 hours, and after the reaction is completed, an antiviral melamine resin material is obtained.

[0045] Example 3

[0046] A method for preparing an antiviral melamine resin material comprises the following steps:

[0047] Step 1, ultrasonically disperse nano titanium dioxide in anhydrous ethanol, and after uniform dispersion, add γ-aminopropyltriethoxysilane, wherein the mass ratio of anhydrous ethanol, nano titanium dioxide and γ-aminopropyltriethoxysilane is 3800:100:95, stir and mix, react at 60°C for 8h, and after the reaction is completed, filter, wash with anhydrous ethanol, and dry in a drying oven at 80°C for 12h to obtain amino titanium dioxide;

[0048] Step 2, ultrasonically dispersing the aminated titanium dioxide in tetrahydrofuran, after uniform dispersion, adding 2,2-dihydroxymethylpropionic acid and dicyclohexylcarbodiimide, stirring and mixing, wherein the mass ratio of aminated titanium dioxide, tetrahydrofuran, 2,2-dihydroxymethylpropionic acid and dicyclohexylcarbodiimide is 100:2000:160:8, reacting at 30°C in a nitrogen atmosphere for 15h, after the reaction is completed, rotary evaporation, vacuum drying at 60°C for 6h, to obtain modified titanium dioxide;

[0049] Step 3, deionized water, modified titanium dioxide and triethanolamine are mixed evenly, heated to 75°C, phosphoric acid is added to adjust the pH to 3, and melamine is added and stirred, wherein the mass ratio of deionized water, modified titanium dioxide, triethanolamine and melamine is 650:8:16:100, and the reaction is carried out at 75°C for 2.5 hours. After the reaction is completed, centrifugation is performed, deionized water is used for washing, and the mixture is dried at 60°C for 12 hours to obtain modified melamine;

[0050] Step 4: Acetone, modified melamine and hexadecane chloride in a mass ratio of 1100:100:85 are stirred and mixed, and reacted at 70° C. for 3.5 hours. After the reaction is completed, the obtained product is precipitated with n-heptane, and then washed with acetone, filtered, and dried to obtain antiviral modified melamine;

[0051] Step 5: Evenly mix a 37% formaldehyde aqueous solution and a 30% sodium hydroxide aqueous solution, adjust the pH value to 8.8, add polyethylene glycol, melamine and antiviral modified melamine, and stir to mix, wherein the mass ratio of the formaldehyde aqueous solution, polyethylene glycol, melamine and antiviral modified melamine is 108:22:100:11, react at 80°C, the reaction time is 2.5 hours, and after the reaction is completed, an antiviral melamine resin material is obtained.

[0052] Example 4

[0053] A method for preparing an antiviral melamine resin material comprises the following steps:

[0054] Step 1, ultrasonically disperse nano titanium dioxide in anhydrous ethanol, and after uniform dispersion, add γ-aminopropyltriethoxysilane, wherein the mass ratio of anhydrous ethanol, nano titanium dioxide and γ-aminopropyltriethoxysilane is 4000:100:102, stir and mix, react at 65°C for 6h, and after the reaction is completed, filter, wash with anhydrous ethanol, and dry in a drying oven at 80°C for 12h to obtain amino titanium dioxide;

[0055] Step 2, ultrasonically dispersing the aminated titanium dioxide in tetrahydrofuran, after uniform dispersion, adding 2,2-dihydroxymethylpropionic acid and dicyclohexylcarbodiimide, stirring and mixing, wherein the mass ratio of aminated titanium dioxide, tetrahydrofuran, 2,2-dihydroxymethylpropionic acid and dicyclohexylcarbodiimide is 100:2100:180:9, reacting at 35°C in a nitrogen atmosphere for 14h, after the reaction is completed, rotary evaporation, vacuum drying at 60°C for 6h, to obtain modified titanium dioxide;

[0056] Step 3, deionized water, modified titanium dioxide and triethanolamine are mixed evenly, heated to 75°C, phosphoric acid is added to adjust the pH to 3, and melamine is added and stirred, wherein the mass ratio of deionized water, modified titanium dioxide, triethanolamine and melamine is 700:9:18:100, and the reaction is carried out at 80°C for 2 hours. After the reaction is completed, centrifugation is performed, deionized water is used for washing, and the mixture is dried at 60°C for 12 hours to obtain modified melamine;

[0057] Step 4: Acetone, modified melamine and hexachlorodecane in a mass ratio of 1200:100:95 are stirred and mixed, and reacted at 75° C. for 3 hours. After the reaction is completed, the obtained product is precipitated with n-heptane, and then washed with acetone, filtered, and dried to obtain antiviral modified melamine;

[0058] Step 5: Evenly mix a 37% formaldehyde aqueous solution and a 30% sodium hydroxide aqueous solution, adjust the pH value to 9.0, add polyethylene glycol, melamine and antiviral modified melamine, and stir to mix, wherein the mass ratio of the formaldehyde aqueous solution, polyethylene glycol, melamine and antiviral modified melamine is 115:24:100:12, react at 85° C., the reaction time is 2 hours, and after the reaction is completed, an antiviral melamine resin material is obtained.

[0059] Comparative Example 1

[0060] A method for preparing a melamine resin material comprises the following steps:

[0061] Step 1, ultrasonically disperse nano titanium dioxide in anhydrous ethanol, and after uniform dispersion, add γ-aminopropyltriethoxysilane, wherein the mass ratio of anhydrous ethanol, nano titanium dioxide and γ-aminopropyltriethoxysilane is 3800:100:95, stir and mix, react at 60°C for 8h, and after the reaction is completed, filter, wash with anhydrous ethanol, and dry in a drying oven at 80°C for 12h to obtain amino titanium dioxide;

[0062] Step 2, ultrasonically dispersing the aminated titanium dioxide in tetrahydrofuran, after uniform dispersion, adding 2,2-dihydroxymethylpropionic acid and dicyclohexylcarbodiimide, stirring and mixing, wherein the mass ratio of aminated titanium dioxide, tetrahydrofuran, 2,2-dihydroxymethylpropionic acid and dicyclohexylcarbodiimide is 100:2000:160:8, reacting at 30°C in a nitrogen atmosphere for 15h, after the reaction is completed, rotary evaporation, vacuum drying at 60°C for 6h, to obtain modified titanium dioxide;

[0063] Step 3, deionized water, modified titanium dioxide and triethanolamine are mixed evenly, heated to 75°C, phosphoric acid is added to adjust the pH to 3, and melamine is added and stirred, wherein the mass ratio of deionized water, modified titanium dioxide, triethanolamine and melamine is 650:8:16:100, and the reaction is carried out at 75°C for 2.5 hours. After the reaction is completed, centrifugation is performed, deionized water is used for washing, and the mixture is dried at 60°C for 12 hours to obtain modified melamine;

[0064] Step 4: Evenly mix a 37% formaldehyde aqueous solution and a 30% sodium hydroxide aqueous solution, adjust the pH value to 8.8, add polyethylene glycol, melamine and modified melamine, and stir to mix, wherein the mass ratio of the formaldehyde aqueous solution, polyethylene glycol, melamine and antiviral modified melamine is 108:22:100:11, react at 80° C., the reaction time is 2.5 hours, and after the reaction is completed, a melamine resin material is obtained.

[0065] Comparative Example 2

[0066] A method for preparing a melamine resin material comprises the following steps:

[0067] Step 1, ultrasonically disperse nano titanium dioxide in anhydrous ethanol, and after uniform dispersion, add γ-aminopropyltriethoxysilane, wherein the mass ratio of anhydrous ethanol, nano titanium dioxide and γ-aminopropyltriethoxysilane is 3800:100:95, stir and mix, react at 60°C for 8h, and after the reaction is completed, filter, wash with anhydrous ethanol, and dry in a drying oven at 80°C for 12h to obtain amino titanium dioxide;

[0068] Step 2, ultrasonically dispersing the aminated titanium dioxide in tetrahydrofuran, after uniform dispersion, adding 2,2-dihydroxymethylpropionic acid and dicyclohexylcarbodiimide, stirring and mixing, wherein the mass ratio of aminated titanium dioxide, tetrahydrofuran, 2,2-dihydroxymethylpropionic acid and dicyclohexylcarbodiimide is 100:2000:160:8, reacting at 30°C in a nitrogen atmosphere for 15h, after the reaction is completed, rotary evaporation, vacuum drying at 60°C for 6h, to obtain modified titanium dioxide;

[0069] Step 3: Evenly mix a 37% formaldehyde aqueous solution and a 30% sodium hydroxide aqueous solution, adjust the pH value to 8.8, add polyethylene glycol, melamine and modified titanium dioxide, and stir to mix, wherein the mass ratio of the formaldehyde aqueous solution, polyethylene glycol, melamine and modified titanium dioxide is 108:22:110:1, react at 80°C for 2.5 hours, and after the reaction is completed, a melamine resin material is obtained.

[0070] Comparative Example 3

[0071] A method for preparing a melamine resin material comprises the following steps:

[0072] Step 1, ultrasonically disperse nano titanium dioxide in anhydrous ethanol, and after uniform dispersion, add γ-aminopropyltriethoxysilane, wherein the mass ratio of anhydrous ethanol, nano titanium dioxide and γ-aminopropyltriethoxysilane is 3800:100:95, stir and mix, react at 60°C for 8h, and after the reaction is completed, filter, wash with anhydrous ethanol, and dry in a drying oven at 80°C for 12h to obtain amino titanium dioxide;

[0073] Step 2, ultrasonically dispersing the aminated titanium dioxide in tetrahydrofuran, after uniform dispersion, adding 2,2-dihydroxymethylpropionic acid and dicyclohexylcarbodiimide, stirring and mixing, wherein the mass ratio of aminated titanium dioxide, tetrahydrofuran, 2,2-dihydroxymethylpropionic acid and dicyclohexylcarbodiimide is 100:2000:160:8, reacting at 30°C in a nitrogen atmosphere for 15h, after the reaction is completed, rotary evaporation, vacuum drying at 60°C for 6h, to obtain modified titanium dioxide;

[0074] Step 3, deionized water, modified titanium dioxide and triethanolamine are mixed evenly, heated to 75°C, phosphoric acid is added to adjust the pH to 3, and melamine is added and stirred, wherein the mass ratio of deionized water, modified titanium dioxide, triethanolamine and melamine is 650:8:16:100, and the reaction is carried out at 75°C for 2.5 hours. After the reaction is completed, centrifugation is performed, deionized water is used for washing, and the mixture is dried at 60°C for 12 hours to obtain modified melamine;

[0075] Step 4: Acetone, modified melamine and hexyl bromide in a mass ratio of 1100:100:85 are stirred and mixed, and reacted at 70° C. for 3.5 hours. After the reaction is completed, the obtained product is precipitated with n-heptane, and then washed with acetone, filtered, and dried to obtain quaternary ammonium salt modified melamine;

[0076] Step 5: Evenly mix a 37% formaldehyde aqueous solution and a 30% sodium hydroxide aqueous solution, adjust the pH value to 8.8, add polyethylene glycol, melamine and quaternary ammonium salt modified melamine, and stir to mix, wherein the mass ratio of the formaldehyde aqueous solution, polyethylene glycol, melamine and antiviral modified melamine is 108:22:100:11, react at 80° C., the reaction time is 2.5 hours, and after the reaction is completed, a melamine resin material is obtained.

[0077] The nano titanium dioxide used in the examples and comparative examples of the present invention was purchased from Darcin Nanotechnology Co., Ltd., with an average particle size of 5-10 nm; polyethylene glycol was purchased from Xilong Chemical Co., Ltd., with a relative molecular mass of 1000; melamine was industrial grade, purchased from Chengdu Yulong Chemical Co., Ltd.; other unspecified reagents were commercially available.

[0078] The melamine resin material prepared in Example 1-4 and Comparative Example 1-3 and the dispersant sodium hexametaphosphate were uniformly mixed to obtain a mixed solution, and a fir wood floor (purchased from Zhejiang Fudeli Wood Industry Co., Ltd., with a specification of 500 mm in length × 60 mm in width × 25 mm in thickness) was immersed in the mixed solution, placed in a vacuum treatment device, and vacuumed for 1 hour with a vacuum degree of -0.095 MPa, and dried to obtain samples 1-7 respectively. The performance of samples 1-7 was tested, and the test results are shown as follows:

[0079] (1) Antibacterial performance test: According to LY / T 1926-2010 "Antibacterial Test Method and Antibacterial Effect of Antibacterial Wood (Bamboo) Flooring", the antibacterial property of the sample was tested by the film method. A certain amount of Staphylococcus aureus and Escherichia coli were inoculated on the surface of the sample to be tested, and the corresponding antibacterial experiment was carried out. After 24 hours of incubation, the number of live bacteria in the sample was detected and the corresponding antibacterial rate was calculated. After 24 hours of incubation, the number of live bacteria of the blank control of Staphylococcus aureus was 3.52×10 4After 24 hours of culture, the number of viable E. coli blank control was 2.89×10 4 , Inhibition rate (%) = (average number of viable bacteria recovered from blank samples - average number of viable bacteria recovered from samples) / average number of viable bacteria recovered from blank samples × 100%. The test results are shown in Table 1:

[0080] Table 1

[0081]

[0082] According to the test results in Table 1, it can be seen that samples 1-4 have excellent antibacterial properties, among which the antibacterial rate of sample 4 against Staphylococcus aureus and Escherichia coli can reach 99.9% after culturing for 24 hours. Quaternary ammonium salt was not introduced into sample 5, and the antibacterial rate was greatly reduced. In sample 6, the modified titanium dioxide was not reacted with melamine first, and quaternary ammonium salt was not introduced, and the antibacterial performance was poor, and the antibacterial rates against Staphylococcus aureus and Escherichia coli were 77.3% and 79.1%, respectively. In sample 7, hexyl bromide was used instead of long-chain halogenated alkane, and the antibacterial performance was reduced, but the impact was small, and the antibacterial rates against Staphylococcus aureus and Escherichia coli were 98.6% and 98.7%, respectively.

[0083] (2) Antiviral performance test: Sample 4 was selected for antiviral performance test. The test standard referred to the test method specified in T / GDTL 011-2020 "Antibacterial and Antiviral Coatings". The test viruses were influenza A virus H3N2 (ATCC VR-1679) and enterovirus EV71 (ATCC VR-1432). The host of influenza A virus H3N2 was MDCK cells; the host of enterovirus EV71 was Vero cells. The experimental group without sample 4 was the control group. The control group and the experimental group corresponding to sample 4 were tested for antiviral performance. The test results are shown in Table 2:

[0084] Table 2

[0085]

[0086] From the test results in Table 2, it can be seen that sample 4 has excellent antiviral properties, and has excellent antiviral capabilities against influenza A virus H3N2 and enterovirus EV71. The virus inactivation rate for influenza A virus H3N2 can reach 97.5%, and the virus inactivation rate for enterovirus EV71 can reach 96.8%.

[0087] (3) Mechanical properties test: Samples 1-7 were placed on a wood-based panel testing machine MWW-10 for the corresponding static bending strength test. At least five samples were tested in each group, and the average test results were taken as shown in Table 3:

[0088] Table 3

[0089]

[0090] From the test results in Table 3, it can be seen that samples 1-4 have excellent mechanical properties, and generate melamine resin materials with cross-linked networks, which greatly improve the intramolecular deformability and the high activity of the molecular chain, thereby reducing the cross-linking density of the resin, increasing the bendability, and improving the flexibility of the resin products. The long-chain alkanes introduced in the process of introducing quaternary ammonium salts can further improve the toughness of the matrix. The corresponding static bending strength of sample 4 can reach 44.5MPa.

[0091] Although the embodiments of the present invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that all equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.

Claims

1. A method for preparing an antiviral melamine resin material, characterized in that: The steps include: Step 1, ultrasonically disperse nano titanium dioxide in anhydrous ethanol, and after uniform dispersion, add γ-aminopropyltriethoxysilane, stir and mix, react, and after the reaction is completed, filter, wash with anhydrous ethanol, and dry in a drying oven at 80° C. for 12 hours to obtain amino titanium dioxide; Step 2: Ultrasonically disperse the amino titanium dioxide in tetrahydrofuran, and after uniform dispersion, add 2,2-dihydroxymethylpropionic acid and dicyclohexylcarbodiimide, stir and mix, and react in a nitrogen atmosphere. After the reaction is completed, rotary evaporate and vacuum dry at 60° C. for 6 hours to obtain modified titanium dioxide; Step 3, deionized water, modified titanium dioxide and triethanolamine are mixed evenly, heated to 75°C, phosphoric acid is added to adjust the pH to 3, and melamine is added, stirred and mixed to react. After the reaction is completed, centrifugation is performed, deionized water is used for washing, and the mixture is dried at 60°C for 12 hours to obtain modified melamine; Step 4: Acetone, modified melamine and hexadecane are stirred and mixed to react. After the reaction is completed, the obtained product is precipitated with n-heptane, and then washed with acetone, filtered, and dried to obtain antiviral modified melamine; Step 5: Evenly mix the formaldehyde solution and the sodium hydroxide solution, adjust the pH value to 8.5-9.0, then add polyethylene glycol, melamine and antiviral modified melamine, stir and mix, react, and after the reaction is completed, obtain the antiviral melamine resin material.

2. The method for preparing an antiviral melamine resin material according to claim 1, characterized in that: In the step 2, the mass ratio of amination titanium dioxide, tetrahydrofuran, 2,2-dihydroxymethylpropionic acid and dicyclohexylcarbodiimide is 100:1500-2100:105-180:5-9, the reaction temperature is 25-35° C., and the reaction time is 14-16 hours.

3. The method for preparing an antiviral melamine resin material according to claim 1, characterized in that: In the step three, the mass ratio of deionized water, modified titanium dioxide, triethanolamine and melamine is 550-700:5-9:12-18:

100.

4. The method for preparing an antiviral melamine resin material according to claim 1, characterized in that: The reaction temperature in step 3 is 70-80° C. and the reaction time is 2-3 h.

5. The method for preparing an antiviral melamine resin material according to claim 1, characterized in that: In the step 4, the mass ratio of acetone, modified melamine and hexadecane chloride is 900-1200:100:68-95.

6. The method for preparing an antiviral melamine resin material according to claim 1, characterized in that: The reaction temperature in step 4 is 65-75° C., and the reaction time is 3-4 h.

7. The method for preparing an antiviral melamine resin material according to claim 1, characterized in that: In the step 5, the mass ratio of the formaldehyde solution, polyethylene glycol, melamine and antiviral modified melamine is 95-115:18-24:100:9-12.

8. The method for preparing an antiviral melamine resin material according to claim 1, characterized in that: The reaction temperature in step 5 is 75-85° C., and the reaction time is 2-3 h.

9. An antiviral melamine resin material prepared by the method for preparing an antiviral melamine resin material according to any one of claims 1 to 8.

10. Use of the antiviral melamine resin material according to claim 9 in indoor furniture panels and floors.

Citation Information

Patent Citations

  • Silver ion inorganic antiseptic and melamine resin and impregnated paper prepared by same

    CN103222477B

  • Antibacterial anti-ultraviolet-ray melamine impregnated paper and preparation method thereof

    CN110438844A

  • Self-antibacterial type high-bonding strength melamine resin adhesive and preparation method thereof

    CN110452645A

  • Functionalized titanium dioxide antibacterial hydrogel and preparation method thereof

    CN113444265A