Flame retardant heat insulating ceramic pad and preparation method thereof
By using flame-retardant and heat-insulated ceramic pads composed of flame-retardant backing layer, inorganic fiber barrier layer and flame-retardant coating layer with specific group distribution ratio in the battery, the problem of poor performance of existing materials at high temperatures is solved, and the problem of poor performance of existing materials at high temperatures is achieved. It has efficient flame retardant and thermal insulation effect and low-cost production, suitable for battery safety applications.
Patent Information
- Application Number
- CN202311326206.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-12
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-10-12
AI Technical Summary
The existing flame retardant insulation materials have poor performance at high temperatures, resulting in frequent battery fire accidents, high manufacturing costs and expensive prices, which cannot effectively prevent and slow down the spread of thermal runaway from the battery cell.
The flame-retardant and heat-insulated ceramic pad consisting of a flame-retardant backing layer, an inorganic fiber barrier layer and a flame-retardant coating layer are used to release moisture and carbon dioxide at high temperatures through the flame-retardant coating layer with a specific group distribution ratio, actively prevent fire and cool down, combined with Multi-layer structure and low thermal conductivity inorganic fibers improve flame retardant and heat insulation.
It realizes the effect of active fire protection and physical heat insulation at high temperatures, reduces flame temperature, significantly improves flame retardant and heat insulation performance, is low-cost, is suitable for large-scale production, and effectively slows down the high temperature spread of chemical batteries in thermal runaway.
Smart Images

Figure CN117384560B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of heat-insulating and fire-proofing products, and in particular relates to a flame-retardant heat-insulating ceramic pad and a preparation method thereof. Background Art
[0002] In recent years, the rapid development of lithium-ion batteries has promoted the prosperity of electric vehicles, energy storage and other fields. However, fire accidents caused by lithium batteries have occurred frequently. In 2022 alone, there were 18,000 fires in electric bicycles and electric power-assisted bicycles, reaching an average of 50 per day. This poses a huge safety hazard to people's production and life.
[0003] In 2020, the Ministry of Industry and Information Technology organized the formulation of the "GB18384-
[0004] The three mandatory national standards, GB38032-2020 Safety Requirements for Electric Vehicles, GB38032-2020 Safety Requirements for Electric Buses, and GB38031-2020 Safety Requirements for Power Batteries for Electric Vehicles, require that while optimizing the safety requirements for battery cells and modules, they also focus on strengthening the thermal safety, mechanical safety, electrical safety, and functional safety requirements for battery systems. In particular, the standard adds a thermal diffusion test for the battery system, requiring that after a thermal runaway occurs in a battery cell, the battery system will not catch fire or explode within 5 minutes, leaving safe escape time for the occupants. Therefore, how to delay and prevent the spread of thermal runaway of battery cells to surrounding cells has become an important safety bottleneck.
[0005] Using appropriate flame-retardant insulation materials to achieve thermal isolation is a relatively mature method. Common flame-retardant insulation materials mainly include: aerogel, foamed silica gel, mica paper, etc. However, foamed silica gel has a low heat resistance and is easily burned through by high temperatures; aerogel has poor strength and is easy to lose powder, so it needs to be reinforced by fiber materials, which increases the manufacturing cost and makes it expensive; mica paper has poor insulation effect.
[0006] To this end, the present invention provides a flame retardant heat insulating ceramic pad and a preparation method thereof. Summary of the invention
[0007] In view of the above problems existing in the prior art, the object of the present invention is to provide a flame retardant and heat insulating ceramic pad and a preparation method thereof, which can improve the flame retardant and heat insulating effects.
[0008] The purpose of the present invention can be achieved by the following technical solutions:
[0009] A flame retardant heat insulating ceramic pad, the flame retardant heat insulating ceramic pad is composed of a flame retardant adhesive layer, an inorganic fiber barrier layer and a flame retardant coating layer, wherein the flame retardant coating layer includes the following parts by weight:
[0010] 20-30 parts of silicate;
[0011] 10-20 parts of borate;
[0012] 1-10 parts of acid;
[0013] Phosphate 5-30 parts;
[0014] 10-50 parts of foaming agent;
[0015] 30-100 parts of water.
[0016] Preferably, the flame retardant thermal insulation ceramic pad includes at least one of a flame retardant polyester film, a flame retardant double-sided adhesive film, a flame retardant polyimide film, a polytetrafluoroethylene film, and a flame retardant kraft paper.
[0017] Preferably, the inorganic fiber barrier layer includes at least one of aluminum silicate fiber, alumina fiber, mullite fiber, basalt fiber, rock wool fiber, slag wool fiber and glass fiber.
[0018] Preferably, the silicate is an alkali metal silicate having a modulus of 1-4.
[0019] Preferably, the borate is an orthoborate containing an alkali metal and an ammonium ion;
[0020] or a metaborate comprising an alkali metal and an ammonium ion;
[0021] or polymeric borates containing alkali metal and ammonium ions.
[0022] Preferably, the phosphate is an orthophosphate containing an alkali metal and an ammonium ion;
[0023] Or the phosphate is a phosphite containing an alkali metal and an ammonium ion;
[0024] Or the phosphate is a hypophosphite containing an alkali metal and an ammonium ion;
[0025] Or the phosphate is an acid salt containing an alkali metal and an ammonium ion;
[0026] Alternatively, the phosphate is a polymeric phosphate containing alkali metal and ammonium ions.
[0027] Preferably, the foaming agent is one or more combinations of magnesium hydroxide, aluminum hydroxide, calcium oxalate and magnesium carbonate.
[0028] The present invention also provides a method for preparing the flame retardant thermal insulation ceramic pad as described above, comprising the following steps:
[0029] S1. Laminating: laminating the flame retardant adhesive layer on the front side of the inorganic fiber barrier layer;
[0030] S2. Prepare a flame retardant coating: weigh each component according to the mass fraction of the flame retardant coating layer, add silicate, borate and phosphate in heated and stirred water in sequence to obtain slurry A; then add acid to slurry A under stirring, and finally add foaming agent powder, and stir evenly to obtain a flame retardant coating;
[0031] S3, coating: the inorganic fiber barrier layer in S1 is placed into a coating machine with the side without adhesive layer facing upward; the flame retardant coating of S2 is evenly coated on the inorganic fiber barrier layer, and then dried in an oven to remove moisture;
[0032] S4, laminating: laminating the flame retardant adhesive layer on the side coated with the flame retardant coating layer in S3 by a laminating machine to obtain a flame retardant thermal insulation ceramic tape;
[0033] S5. Die-cutting: according to the required size and specifications, cut the flame-retardant and heat-insulating ceramic tapes coated on both sides into the required flame-retardant and heat-insulating ceramic pads.
[0034] Preferably, the temperature range of heating by the heater in step S2 is 50-100° C.; the speed range of stirring by the stirrer in step S2 is 100-1000 rpm.
[0035] Preferably, the thickness of the flame retardant coating in step S3 is in the range of 0.1-2 mm, and the drying temperature is in the range of 80-150°C.
[0036] As described above, the flame retardant and heat insulating ceramic pad and the preparation method thereof provided by the present invention have the following beneficial effects:
[0037] (1) The flame-retardant heat-insulating ceramic pad of the present invention is prepared by using a specific composition ratio of the flame-retardant coating by mass. When subjected to heating, high temperature or open flame, it is thermally decomposed to release water and carbon dioxide, which can absorb a large amount of heat from the heat source, and can actively prevent fires. In addition to the role of physical insulation, it can also play a role in actively cooling and extinguishing fires;
[0038] (2) The flame retardant and heat insulating ceramic pad of the present invention has a multi-layer structure, and the thermal conductivity of the inorganic fiber barrier layer is low. At the same time, it has the properties of high temperature resistance and heat insulation. As a base material of the flame retardant coating, it complements the flame retardant coating and greatly improves the flame retardant and heat insulating effect;
[0039] (3) The process of the present invention is simple, low-cost, and suitable for large-scale batch production; the product has good fire retardant effect and can effectively slow down the spread of high temperature caused by thermal runaway of chemical batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 A preparation flow chart of Example 1 in the application for a flame retardant and heat insulating ceramic pad of the present invention;
[0041] Figure 2Schematic diagram of an optical microscope of a sample prepared in Example 1 of the present application;
[0042] Figure 3 This is a curve diagram of the change in back temperature of the sample prepared in Example 1 of the present application when burned by an alcohol lamp flame;
[0043] Figure 4 A flow chart for preparing a double-sided coated sample of Example 2 in the flame retardant and heat insulating ceramic pad of the present invention;
[0044] Figure 5 Schematic diagram of an optical microscope of a sample prepared in Example 2 of the present application;
[0045] Figure 6 This is a curve diagram of the back surface temperature change of the sample prepared in Example 2 of the present application measured under the hot stage;
[0046] Figure 7 This is a curve diagram of the change in back surface temperature of the sample prepared in Example 2 of the present application when burned by an alcohol lamp flame;
[0047] Figure 8 This is a thermal effect curve of the sample prepared in Example 3 of the present application measured by a differential scanning calorimeter;
[0048] Fig. 9 This is a curve diagram of the change in back surface temperature of a 2.5 mm thick carbon fiber aerogel sheet of Comparative Example 1 of the present application when burned by an alcohol lamp flame;
[0049] Fig.10 This is a thermal effect curve of a 2.5 mm thick carbon fiber aerogel sheet of Comparative Example 1 of the present application measured by a differential scanning calorimeter;
[0050] Fig.11 This is a curve chart of the temperature change on the back side of the 3 mm thick aluminum silicate fiber blanket of Comparative Example 2 of the present application when burned by an alcohol lamp flame. DETAILED DESCRIPTION
[0051] The following is a description of the implementation of the present invention by means of specific embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification.
[0052] Example 1
[0053] The present embodiment provides a flame retardant thermal insulation ceramic pad, which consists of a flame retardant adhesive layer, an inorganic fiber barrier layer and a flame retardant coating layer; wherein the flame retardant adhesive layer is a flame retardant double-sided tape and a flame retardant polyester film, and the inorganic fiber barrier layer is mullite fiber; the raw materials of the flame retardant coating layer are: 20 parts of sodium silicate water glass (modulus 1.5), 10 parts of sodium borate, 8 parts of phosphoric acid, 5 parts of sodium phosphate, 20 parts of foaming agent magnesium hydroxide, and 80 parts of water.
[0054] See the preparation flow chart for Figure 1 As shown, the preparation method of the flame retardant thermal insulation ceramic pad comprises the following steps:
[0055] S1. Laminating: Laminating the flame retardant polyester film on the front side of the mullite fiber barrier layer with a thickness of about 2 mm;
[0056] S2. Prepare flame retardant coating: weigh each component according to the mass parts, preheat 80 parts of water to 60° C. using a heater, add sodium silicate water glass, sodium borate and sodium phosphate in sequence at a stirring speed of 300 rpm using a stirrer, and obtain slurry A after dissolution; then continue stirring, add phosphoric acid to slurry A, and finally add foaming agent powder magnesium hydroxide, and stir evenly to obtain flame retardant coating;
[0057] S3, coating: Place the mullite fiber barrier in S1 with the side without adhesive layer facing upwards, and send it into a PTX-600 small coating machine, use a scraper coating, control the gap height to 0.8mm, and the speed to 1m / min, and evenly coat the flame retardant coating prepared in S2 on the inorganic fiber barrier layer, and dry it in an oven at 120°C for 5min to remove moisture, and obtain a dry coated tape;
[0058] S4, laminating: laminating the flame retardant double-sided tape on one side coated with the flame retardant coating layer in S3 by a laminating machine to obtain a flame retardant thermal insulation ceramic tape;
[0059] S5. Die-cutting: Use a die-cutting machine to cut the flame-retardant thermal insulation ceramic tape into the required flame-retardant thermal insulation ceramic pad finished products.
[0060] The optical microscope photo of the obtained flame retardant thermal insulation ceramic can be found at Figure 2 As shown; wherein a is a flame retardant double-sided adhesive, b is a flame retardant coating layer, c is a mullite fiber layer, and d is a flame retardant polyester film.
[0061] Tear off the flame-retardant double-sided adhesive release paper on the a side of the flame-retardant thermal insulation ceramic pad, and use 3 K-type thermocouples to stick on the flame-retardant thermal insulation ceramic pad to measure the temperature; and use the flame of an alcohol lamp to directly burn the flame-retardant polyester film on the d side, and measure the temperature change of the a side in real time. The results can be found in Figure 3 As shown; combined with Table 1, it can be seen that the flame of the alcohol lamp continues to burn for 10 minutes, and the maximum temperature of surface a does not exceed 210°C, showing good flame retardant and heat-insulating properties; compared with the existing ones, the flame retardant and heat-insulating effect of the flame retardant and heat-insulating ceramic pad can be improved.
[0062] Example 2
[0063] The present embodiment provides a flame retardant thermal insulation ceramic pad, which consists of a flame retardant adhesive layer, an inorganic fiber barrier layer and a flame retardant coating layer; wherein the flame retardant adhesive layer is a flame retardant double-sided tape, and the inorganic fiber barrier layer is aluminum silicate fiber; the raw materials of the flame retardant coating layer are: 20 parts of potassium silicate water glass (modulus 2), 15 parts of potassium borate, 10 parts of sulfuric acid, 15 parts of sodium polyphosphate, 10 parts of basic magnesium carbonate as a foaming agent, and 100 parts of water.
[0064] See the preparation flow chart for Figure 4 As shown, the preparation method of the flame retardant thermal insulation ceramic pad comprises the following steps:
[0065] S1. Prepare flame retardant coating: weigh each component according to the mass parts, preheat 100 parts of water to 80° C. using a heater, add potassium silicate water glass, potassium borate, and sodium polyphosphate in sequence using a stirrer at a stirring speed of 300 rpm, and stir to obtain slurry A; then continue stirring, add sulfuric acid to slurry A, and finally add foaming agent powdered basic magnesium carbonate, and stir evenly to obtain flame retardant coating;
[0066] S2, coating: feed aluminum silicate fiber with a thickness of about 0.75 mm into a small coating machine of type PTX-600, adopt scraper coating, control the gap height to 0.6 mm, and the speed to 1 m / min, and evenly coat the flame retardant coating prepared in S1 on the inorganic fiber barrier layer, and dry it in an oven at 110°C for 6 minutes to remove moisture, and obtain a dry single-sided coated tape;
[0067] S3, laminating: laminating the flame retardant double-sided tape on one side coated with the flame retardant coating layer in S2 through a laminating machine to obtain a single-sided flame retardant thermal insulation ceramic tape;
[0068] S4, secondary coating: the flame retardant thermal insulation ceramic tape coated on one side obtained in S3 is fed into a PTX-600 small coating machine again, with the aluminum silicate fiber without coating facing upward, and the fiber is continuously coated with a scraper, with the gap height controlled at 0.6 mm and the speed at 1 m / min, and then dried in an oven at 110° C. for 6 min to remove moisture, and obtain a dry coated tape;
[0069] S5, secondary coating: coating the side coated with the flame retardant coating layer in S4 by adopting the steps similar to S3, so as to obtain a flame retardant heat insulating ceramic tape coated on both sides;
[0070] S6. Die-cutting: Use a die-cutting machine to cut the flame-retardant thermal insulation ceramic tape into the required flame-retardant thermal insulation ceramic pad finished products.
[0071] The optical microscope photo of the obtained flame retardant thermal insulation ceramic pad can be found at Figure 5 As shown, a is a flame retardant double-sided adhesive, b is a flame retardant coating layer, and c is an aluminum silicate fiber layer; the total thickness of the flame retardant thermal insulation ceramic pad is about 1.6 mm.
[0072] Tear off the flame-retardant double-sided adhesive release paper on the a side of the obtained flame-retardant thermal insulation ceramic pad, and use two K-type thermocouples to stick on the flame-retardant thermal insulation ceramic pad to measure the temperature; stick the flame-retardant thermal insulation ceramic pad on a hot table, and raise the temperature to 300°C and maintain it; measure the temperature change on the back of the flame-retardant thermal insulation ceramic pad in real time, and the results are shown in Figure 6 As shown; it can be seen that when the hot surface temperature is maintained for 20 minutes, the maximum temperature of the back side does not exceed 160°C, showing good flame retardant and heat-insulating properties; compared with the existing ones, the flame retardant and heat-insulating effect of the flame retardant and heat-insulating ceramic pad can be improved.
[0073] The flame retardant double-sided adhesive release paper on the a side of the flame retardant thermal insulation ceramic pad was torn off, and three K-type thermocouples were pasted on the flame retardant thermal insulation ceramic pad to measure the temperature. The flame of an alcohol lamp was used to directly burn the flame retardant double-sided adhesive on the other side, and the temperature change of the cold side was measured in real time. The results are shown in Figure 7 As shown; combined with Table 1, it can be seen that when the alcohol lamp flame continues to burn for 10 minutes, the maximum temperature of the cold surface does not exceed 230°C, showing good flame retardant and heat-insulating properties; compared with the existing ones, the flame retardant and heat-insulating effect of the flame retardant and heat-insulating ceramic pad can be improved.
[0074] Example 3
[0075] This embodiment provides a flame retardant thermal insulation ceramic pad, which is composed of a flame retardant adhesive layer, an inorganic fiber barrier layer and a flame retardant coating layer; similarly, its specific composition and preparation process are the same as in Example 2. The flame retardant double-sided adhesive release paper on both sides of the obtained flame retardant thermal insulation ceramic pad is torn off, and then the thermal effect is measured using a STA449 differential scanning calorimeter produced by NETZSCH in Germany; the temperature is raised to 1000°C at a rate of 10°C / min in a nitrogen atmosphere, and the results are shown in Figure 8 As shown. It can be seen that during the heating process, obvious endothermal peaks appeared at 100-200℃ and 200-400℃ respectively; due to the heat absorption of the flame retardant thermal insulation ceramic pad during the heating process, it plays an active cooling role, which can well reduce the temperature of the flame and achieve a better flame retardant and thermal insulation effect; compared with the existing ones, the flame retardant and thermal insulation effect of the flame retardant thermal insulation ceramic pad can be improved.
[0076] Comparative Example 1
[0077] After removing the plastic sealing PET film from the surface of a 2.5mm thick carbon fiber aerogel sheet, three K-type thermocouples were attached to the surface of the carbon fiber aerogel sheet with flame retardant double-sided tape to measure the temperature; the other side of the aerogel was directly burned with an alcohol lamp flame, and the temperature change of the cold side was measured in real time. The results can be found in Fig. 9As shown; it can be seen that under the heating of the alcohol lamp flame, the temperature of the cold surface of the carbon fiber aerogel rises rapidly, reaching a maximum temperature of 265°C in 3 minutes; while the maximum temperatures of the flame retardant and thermal insulation ceramic pad samples in Example 1 and Example 2 are 140°C and 110°C in 3 minutes, respectively, which are significantly lower than those of the carbon fiber aerogel; this indicates that the flame retardant and thermal insulation ceramic pad of the present invention has better flame retardant and thermal insulation properties.
[0078] The thermal effect of the carbon fiber aerogel sheet with a thickness of 2.5 mm was measured using a STA449 differential scanning calorimeter produced by NETZSCH, Germany. In a nitrogen atmosphere, the temperature was raised to 1000°C at a rate of 10°C / min. The results are shown in Fig.10 As shown; it can be seen that in the range of room temperature to 1000°C, the aerogel sheet did not show obvious endothermal effect, and no obvious endothermal peak was detected; this shows that aerogel can only play a physical insulation effect.
[0079] Comparative Example 2
[0080] A K-type thermocouple was attached to a 3mm thick aluminum silicate fiber blanket with flame-retardant double-sided tape to measure the temperature; the other side of the aerogel was directly burned with an alcohol lamp flame, and the temperature change of the cold side was measured in real time. The results are shown in Fig.11 As shown; it can be seen that under the heating of the alcohol lamp flame, the cold surface temperature of the aluminum silicate fiber blanket rises rapidly, reaching a maximum temperature of 310°C in 2 minutes; combined with Table 1, it can be seen that the maximum temperatures of the flame retardant and thermal insulation ceramic pad samples in Example 1 and Example 2 are 140°C and 110°C in 3 minutes, respectively, which are significantly lower than the carbon fiber aerogel, indicating that the flame retardant and thermal insulation ceramic pad of the present invention has better flame retardant and thermal insulation properties.
[0081] Table 1 shows the temperature values of the back of different samples under the burning of alcohol lamp
[0082]
[0083] It should be noted that the data in Example 3 are not included in Table 1.
[0084] The flame retardant heat insulating ceramic pad and the preparation method thereof of the present invention can improve the flame retardant heat insulating effect, which is better than the aerogel products in the prior art (appearing on the market). The flame retardant heat insulating ceramic pad and the preparation method thereof of the present invention are applicable to a variety of chemical power sources, electrical equipment, and electronic equipment.
[0085] The above is only a preferred embodiment of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, which are also considered as the protection scope of the present invention.
Claims
1. A flame retardant thermal insulation ceramic pad, characterized in that: The flame retardant heat insulating ceramic pad is composed of a flame retardant adhesive layer, an inorganic fiber barrier layer and a flame retardant coating layer, wherein the flame retardant coating layer is calculated in the following parts by weight: 20-30 parts of silicate; 10-20 parts of borate; 1-10 parts of acid; Phosphate 5-30 parts; 10-50 parts of foaming agent; 30-100 parts water; The silicate is an alkali metal silicate having a modulus of 1-4; The borate is an orthoborate containing an alkali metal and ammonium ions; or a metaborate containing an alkali metal and ammonium ions; or a polymeric borate containing an alkali metal and ammonium ions; The phosphate is an orthophosphate containing an alkali metal and ammonium ions; or the phosphate is a phosphite containing an alkali metal and ammonium ions; or the phosphate is a hypophosphite containing an alkali metal and ammonium ions; or the phosphate is an acid salt containing an alkali metal and ammonium ions; or the phosphate is a polyphosphate containing an alkali metal and ammonium ions; The foaming agent is one or more combinations of magnesium hydroxide, aluminum hydroxide, calcium oxalate and magnesium carbonate.
2. The flame retardant heat insulating ceramic pad according to claim 1, characterized in that: The flame retardant heat insulating ceramic pad includes at least one of a flame retardant polyester film, a flame retardant double-sided adhesive film, a flame retardant polyimide film, a polytetrafluoroethylene film, and a flame retardant kraft paper.
3. The flame retardant heat insulating ceramic pad according to claim 1, characterized in that: The inorganic fiber barrier layer includes at least one of aluminum silicate fiber, aluminum oxide fiber, mullite fiber, basalt fiber, rock wool fiber, slag wool fiber, and glass fiber.
4. A method for preparing the flame retardant thermal insulation ceramic pad according to any one of claims 1 to 3, characterized in that: The production steps include: S1. Laminating: laminating the flame retardant adhesive layer on the front side of the inorganic fiber barrier layer; S2. Configure flame retardant coating: Weigh the components by mass of the flame retardant coating layer according to claim 1, add silicate, borate and phosphate in heated and stirred water in sequence to obtain slurry A; then add acid to slurry A under stirring, and finally add foaming agent powder, stir evenly to obtain flame retardant coating; S3, coating: the inorganic fiber barrier layer in S1 is placed into a coating machine with the side without adhesive layer facing upward; the flame retardant coating of S2 is evenly coated on the inorganic fiber barrier layer, and then dried in an oven to remove moisture; S4, laminating: laminating the flame retardant adhesive layer on the side coated with the flame retardant coating layer in S3 by a laminating machine to obtain a flame retardant thermal insulation ceramic tape; S5. Die-cutting: according to the required size and specifications, cut the flame-retardant and heat-insulating ceramic tapes coated on both sides into the required flame-retardant and heat-insulating ceramic pads.
5. The method for preparing the flame retardant heat insulating ceramic pad according to claim 4, characterized in that: The temperature range of heating by the heater in step S2 is 50-100° C.; the speed range of stirring by the stirrer in step S2 is 100-1000 rpm.
6. The method for preparing the flame retardant heat insulating ceramic pad according to claim 4, characterized in that: The thickness of the flame retardant coating in step S3 is in the range of 0.1-2 mm, and the drying temperature is in the range of 80-150°C.
Citation Information
Patent Citations
Foaming heat insulation flame retardant solution
CN101597500A
Heat insulation inorganic coating and preparation method thereof
CN104609825A
Silicon-based fire retardant
CN105218863A
Preparation method of phosphate gum-based flame-retardant heat-insulating coating highly ceramic in case of fire
CN115433479A
Flame-retardant nonwoven fabric and filter including the same
JP2009046776A